0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Mechanism

Identifying the mechanism of a ceramic glaze recipe is the key to moving adjusting it, fixing it, reverse engineering it, even avoiding it!

Key phrases linking here: mechanisms, mechanism - Learn more

Details

Identifying a mechanism means you identify the reason a glaze does something specific. Especially visual. Most glaze recipes can be separated into two parts: the base and the mechanism of the color, opacity, and variegation. The base is likely just a transparent glossy or translucent matte (although we can also go to a deeper level and talk about the mechanism of the matteness of a glaze, for example). Most often, a 'base glaze with variations' model is the best way to build a suite of glazes or transfer them to another temperature. A base glaze that is 'understood' can be improved over time, made more and more functional and easier-to-use, less and less mysterious, and prone to problems. When this base is improved, variations based on it benefit also. Imagine a base that is nice to use and apply; never cracks on drying; does not settle out; is reliable; cost-effective; resistant to leaching, crazing, and cutlery marking; is gloss and temperature adjustable; and is easily opacified, colored, and variegated, etc. Would it not make good sense, where possible, to transplant the 'mechanisms' from new glaze recipes into your base rather than parachute the whole recipe (with its new materials and problems) into your operation?

Again, the 'mechanism' of a glaze is the particular material(s) or process(es) that make it do the special visual thing it does. For example, consider a glossy white: it is likely just a glossy transparent base with added zircopax or tin. If you already have a glossy glaze that has the above benefits, then why not just put the opacifier into it?

Consider the mechanism of matteness. A glaze recipe might fire matte because:

-It has a high alumina:silica ratio and the alumina stiffens the melt so that the microsurface is rippled.
-It is not being fired high enough to melt properly.
-It is covered with a fine mesh of crystals that grow during cooling.

Knowing something about the mechanism of a glaze will give you direction if you need to make adjustments. For example, to make an under-fired matte glossier you add feldspar, to make an alumina matte glossier you add silica, to make a crystal matte glossier you cool more quickly or increase kaolin to stiffen the melt and impede crystal growth.

Consider a fairly complex mechanism: A copper red glaze. It is a low alumina, high melt fluidity glaze with a little copper and tin and fired in reduction on a low iron body. Within this system, you can introduce a little boron to move the color toward purple. Knowing this will go a long way to troubleshooting and adjusting it. But moving the mechanism to another fluid base to fire at a lower temperature, for example, will be less practical; it would be better to adjust the chemistry of the source recipe by adding more flux.

Consider another benefit of knowing 'mechanisms'. In the past, you may have mixed recipes from others or textbooks without regard to the mechanism at play in recipes and firing. But when you understand, you see recipes differently and make more educated judgments about whether you want them in your operation. Consider reactive glazes, glazes that really dance with variegations in color and opacity. We know that it is normal for a middle temperature glaze to have 20-30% boron frit to get a good melt (about 0.3 molar equivalents of B2O3). But if you see a glaze that contains 50-60% frit (0.6 molar), a red light should to turn on; this is really going to melt a lot. And it is going to be very particular about thickness, cooling in the kiln, and the contours of ware you put it on. Knowing this upfront is very important to saving yourself a lot of headaches and disappointments. Like copper-reds, this type of glaze cannot really be broken into a base and a mechanism, the fluid nature of the base coupled with the colorants combine to form the visual character.

Some mechanisms live within narrow confines of firing temperature, process and applications methods. An example is a cone 10R dolomite matte. These glazes have around 0.4 molar equivalents of MgO (very high) in a fluid low silica base whose fluxes are dominated by CaO. The fired glass contains phase changes these produce the silky surface texture. Fiddling with the amount of MgO or the material which sources it is going to affect the character of the fired surface. Changing the SiO2:Al2O3 ratio will likewise have an impact. Or the source of the CaO.

Reverse engineering a glaze is a task where it is particularly important to identify mechanisms. It is not just a matter of having the chemistry of a glaze analyzed and expecting that a calculated mix of materials that supplies the same chemistry will fire with the same result. That is wishful thinking! Because so many factors can be at play. It is crystallizing on cooling? Does the color suggest a colorant or mix of colorants that requires a particular type of chemistry in the base? Or does the glaze surface suggest a particular cooling curve? Will it likely only work on a particular body type and why? How much melt fluidity does it need to have and from what flux should it get this? Does it contain entrained bubbles suggesting raw sources of calcia or magnesia were used? Does it have faults (like crazing) that suggest it contains high-soda materials? Etc. There can be so many factors that play to produce the color, surface texture, matteness, speckle, variegation, etc. For variegation, especially, it can be very hard to identify the precise mechanism. How much of the fired appearance derives from the manner of firing, the mineralogy or other physical characteristics of the materials (e.g. particle size), the method of application, etc. Identifying the exact mix of coloring oxides is not always easy, even if you were to have an analysis done (few labs know how to measure ceramic oxides, like boron, well; each oxide has its own analysis idiosyncrasies, and there can be a lot of elements in a glaze). Glazes that contain unusual frits or mixtures that include special-purpose frits will likely be very difficult to duplicate chemically until the right frit has been located. Also, glazes that contain Li2O or BaO from a frit will not behave the same if you supply these oxides from raw materials.

In the end, seeing the mechanisms of a glaze will involve experience and the ability you have built to separate the visual presence of the glaze into the likely recipe, material, process, and chemistry factors that are likely contributors. It can be quite simple in many cases but very complicated in others.

Related Information

Three visual glaze mechanisms make this piece unique


This picture has its own page with more detail, click here to see it.

"Mechanisms" are specifics about the glaze application or preparation process, the materials, the chemistry or firing schedule that produce a specific visual effect. This is fired at cone 10R. It is made from a buff stoneware, Plainsman H550, and has L3954N black engobe on the inside and part way down the outside. The transparent glaze on the inside gives the black a deep vibrant effect. The outside glaze is G2571A with 3.5% rutile and 10% zircopax added (the latter imparts opacity and the former produces the variegated surface). The powerful color of the black engobe wants to get through but it is only able to do so where the glaze layer is thinner (producing the varied shades of brown with differing thicknesses of glaze that occur because of the presence of the incised design).

How do you turn a transparent glaze into a white?


This picture has its own page with more detail, click here to see it.

Right: Ravenscrag GR6-A transparent base glaze. Left: It has been opacified (turned opaque) by adding 10% Zircopax. This opacification mechanism can be transplanted into almost any transparent glaze. It can also be employed in colored transparents, it will convert their coloration to a pastel shade, lightening it. Zircon works well in oxidation and reduction. Tin oxide is another opacifier, it is much more expensive and only works in oxidation firing.

Glaze recipes online waiting for a victim to try them!


A pile of printed recipes to try, but few are likely to work

This picture has its own page with more detail, click here to see it.

You found some recipes. Their photos looked great, you bought $500 of materials to try them, but none worked! Why? Consider these recipes. Many have 50+% feldspar/Cornwall/nepheline (with little dolomite or talc to counteract their high thermal expansion, they will craze). Many are high in Gerstley Borate (it will turn the slurry into a bucket of jelly, cause crawling). Others waste high percentages of expensive tin, lithium and cobalt in crappy base recipes. Metal carbonates in some encourage blistering. Some melt too much and run onto the kiln shelf. Some contain almost no clay (they will settle like a rock in the bucket). A better way? Find, or develop, fritted, stable base transparent glossy and matte base recipes that fit your body, have good slurry properties, resist leaching and cutlery marking. Identify the mechanisms (colorants, opacifiers and variegators) in a recipe you want to try and transplant these into your own base (or mix of bases). And use stains for color (instead of metal oxides).

Additions of iron oxide are coloring, fluxing and crystallizing this base transparent


Glazes range from celadon to heavy iron crystal surface

This picture has its own page with more detail, click here to see it.

Iron oxide is an amazing glaze addition in reduction. Here, I have added it to the G1947U transparent base. It produces green celadons at low percentages. Still transparent where thin, 5% produces an amber glass (and the iron reveals its fluxing power). 7% brings opacity and tiny crystals are developing. By 9% color is black where thick, at 11% where thin or thick - this is “tenmoku territory”. 13% has moved it to an iron crystal (what some would call Tenmoku Gold or Teadust), 17% is almost metallic. Past that, iron crystals are growing atop others. These samples were cooled naturally in a large reduction kiln using the C10RPL firing schedule, the crystallization mechanism would be heavier if it were cooled more slowly (or less if cooled faster). The 7% one in this lineup is quite interesting, a minimal percentage of cobalt-free black stain could likely be added to create an inexpensive and potentially non-leaching jet-black glossy.

A magnesia matte that breaks on contours


This picture has its own page with more detail, click here to see it.

GR10-G Silky magnesia matte cone 10R (Ravenscrag 100, Talc 10, Tin Oxide 4). This is a good example silky matte mechanism of high MgO. The Ravenscrag:Talc mix produces a good silky matte, the added tin appears to break the effect at the edges.

The mechanism of Cd, Se stain inclusion


This picture has its own page with more detail, click here to see it.

Glossy blacks are best made adding a black stain to a quality base transparent


This picture has its own page with more detail, click here to see it.

The glaze on the left is called Tenmoku Cone 6 (a popular, and old, CM recipe). It is 20% calcium carbonate, 35% Custer feldspar, 15% OM4 Ball Clay and 30% silica, 10% iron oxide. If you have any experience with glaze you will note two things that a fishy here: There is no boron, lithia or zinc sourcing material. How can this melt enough at cone 6? It looks melted, but the ease of scratching it shows it is not. So, it appears that if we saturate an incompletely melted glaze with a lot of refractory brown colorant on a dark body the effect can be black. A better idea is the glaze on the right. We start with a stable, reliable base transparent, G2926B. Then we add 5% Mason 6666 black stain (stains are smelted at high temperatures, quenched and ground, they are inert and relatively safe). A bonus is we end up with a slurry that is not nearly as messy to use and does not turn into a bucket of jelly.

The rutile mechanism in glazes


This picture has its own page with more detail, click here to see it.

2, 3, 4, 5% rutile added to an 80:20 mix of Alberta Slip:Frit 3134 at cone 6. This variegating mechanism of rutile is well-known among potters. Rutile can be added to many glazes to variegate existing color and opacification. If more rutile is added the surface turns an ugly yellow in a mass of titanium crystals.

Comparing two glazes having different mechanisms for their matteness


This picture has its own page with more detail, click here to see it.

These are two cone 6 matte glazes (shown side by side in an account at Insight-live). G1214Z is a calcia matte, it has a high silica:alumina ratio. It crystallizes during cooling to make the matte effect. Melt fluidity is needed for that and this GLFL test shows that it certainly has that. The degree of matteness is adjustable by tuning the SiO2 content. The G2928C is a magnesia matte, it has high MgO and produces the classic silky micro-wrinkled the surface. Its matteness is adjustable by trimming the calcined kaolin. CaO is a standard oxide that is in almost all glazes, 0.4 is not high for it. But much less MgO is needed for it to make a matte. The G2928C also has 5% tin, if that was not there it would be darker than the other one because Ravenscrag Slip has some iron. This glaze actually has texture like a dolomite matte at cone 10R, it is great. And it has wonderful application properties. And it does not craze, on Plainsman M370 (it even survived a 300F-to-ice water IWCT test). This looks like it could be a great liner glaze.

A breaking glaze highlights incised decoration:

The mechanism is variation in thickness


This picture has its own page with more detail, click here to see it.

This is the Ravenscrag slip cone 6 base (GR6-A which is 80 Ravenscrag, 20 Frit 3134) with 10% Mason 6006 stain (our code GR6-L). Notice how the color is white where it thins on contours, this is called "breaking". Thus we say that this glaze "breaks to white". The development of this color needs the right chemistry in the host glaze, and it needs depth to work (on the edges the glaze is too thin so there is no color). The breaking phenomenon has many mechanisms; this is just one. Interestingly, the GR6-A transparent base has more entrained micro-bubbles than a frit-based glaze; however, these enhance the color effect in this case.

In pigmented glossy transparent glazes

The pigment is the opacifier


This picture has its own page with more detail, click here to see it.

This is a cone 6 oxidation transparent glaze having enough flux (from a boron frit) to make it melt very well, that is why it is running and pooling. Iron oxide has been added (around 5%), producing this transparent amber effect. Darker coloration occurs where the glaze has run thicker (because it absorbs more light). This simple mechanism enables the glaze to automatically highlight contours, emboss and textures on the underlying surface. This mechanism works with any color in almost any transparent base glaze, as long as bubble clouding and crystallization do not occur. Entire lines of commercial glazes (e.g. AMACO Celadons) are based on this mechanism and potters prize it (industry doesn't like it because it is difficult to achieve consistency).

This glaze relies on high levels of K2O and Na2O to produce the brilliant gloss, however the side effect of that is crazing. These are sourced by feldspars, nepheline syenite and are high in certain frits. To achieve this effect, recipes must rely on other fluxes like boron, lithium or zinc.

Cone 6 glaze speckling mechanism


This picture has its own page with more detail, click here to see it.

This cone 6 white opacified glaze has an addition pigment-bearing granular mineral to create speckle (e.g. illmenite, manganese granular, ironstone concretions). This speckling mechanism can be transplanted into almost any glaze. Unfortunately, the metallic particles that produce the speck are often heavy and settle quickly in the glaze slurry. This can be prevented somewhat by flocculating the slurry.

Inbound Photo Links



Pure Nepheline Syenite as a crackle glaze: Its chemistry explains exactly why crackle glazes crack

Links

Glossary Limit Recipe
"Recipe logic" is the ability to sanity-check ceramic glaze recipes on sight, by noting that materials present and their relative percentages.
Glossary Opacity
Opacity of ceramics glazes is normally achieved by adding an opacifier like tin oxide or zircon. However, there are chemical profiles that can turn transparent glazes milky and make it cheaper to opacify them.
Projects Troubles
Articles Where do I start in understanding glazes?
Break your addiction to online recipes that don't work or bottled expensive glazes that you could DIY. Learn why glazes fire as they do. Why each material is used. How to create perfect dipping and brushing properties. Even some chemistry.
Properties Glaze Variegation

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy