Glaze opacity refers to the degree to which it is opaque. Opacifiers are powders added to transparent ceramic glazes to make them opaque.
Key phrases linking here: opacification, opacifiers, opacifier, opacify - Learn more
A glaze additive that impart opacity, transforming an otherwise transparent glaze into an opaque one. Common opacifiers are tin oxide and zircon compounds. Opacifiers typically work by simply not dissolving into the melt, the white suspended particles thus reflect and scatter the light. Since they do not participate in the chemistry of the melt, they are typically rationalized at the recipe level (their effect on thermal expansion, development of colors and glaze hardness are obvious factors).
Another mechanism of opacity is crystallization, which can occur when a crystallizing ingredient is supersaturated into the mix (e.g. TiO2) or when slow cooling a glaze to encourage crystallization of less saturated oxides that crystallize easily (e.g. boron blue). This mechanism is more likely to produce a glass that cutlery marks.
A third mechanism is suspended micro-bubbles that cloud the glass. These are often candidates for being able to use lower opacifer percentages.
Opacified glazes can be more subject to cutlery marking. This is especially the case when a glaze is simply not melting to as smooth a surface. The addition of refractory zircon opacifier is a case in point: Jagged edges of microscopic particles can protrude out of the surface.
When opacifiers are added to pigmented glazes, color depth and intensity are lost. However, consistency of color is gained because changes in thickness are less prone to changes in tone or intensity. A disadvantage of pacifying color glazes is that higher percentages of stain are needed to get intense color.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. The tin is on the right.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. Of course, rutile could be used in place of titanium; it contains iron oxide that would enhance the development of blue. A small amount of cobalt can also be added to enhance the blue (the G2934 magnesia matte on the left, especially, will respond to that).

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS.

This picture has its own page with more detail, click here to see it.
Right: Ravenscrag GR6-A transparent base glaze. Left: It has been opacified (turned opaque) by adding 10% Zircopax. This opacification mechanism can be transplanted into almost any transparent glaze. It can also be employed in colored transparents, it will convert their coloration to a pastel shade, lightening it. Zircon works well in oxidation and reduction. Tin oxide is another opacifier, it is much more expensive and only works in oxidation firing.

This picture has its own page with more detail, click here to see it.
This sanitary ware tank lid was made in China. Notice how thick the white glaze is being applied to cover the iron containing body below. This is a testament to how opaque a zircon opacified glaze can be. Zircon often causes crawling (likely due to a combination of the effects of its fine particle size on drying properties and its tendency to stiffen the melt). Extra measures and constant attention to detail (e.g. glaze thickness, slurry rheology, avoidance of sharp contours on ware) are needed with such glazes.

This picture has its own page with more detail, click here to see it.
This is a lithium glaze fired at cone 6. It has 6% titanium. This effect will also work in other types of transparent recipes. There should be more blue with slower cooling. Mixing some rutile in (e.g. 4 titanium, 2 rutile) should enhance also. 6% is pushing the edge of how much titanium should be in a recipe. Any more, or cooling too slow, could transform the surface into a mass of white crystals (which would be rough and non-functional). It is best to manually program firings, the up and down schedules? That would make the result consistent no matter how heavily or lightly loaded a kiln is.

This picture has its own page with more detail, click here to see it.
This is a cone 04 glaze on a terra cotta body. Two 300-gram test batches were made. Both have 5% tin oxide added to a base transparent, G1916Q. The one on the left was high-speed propeller-mixed for 10 seconds. That was not enough, small agglomerates appear as tiny white specks floating in the glass. The one on the right was blender mixed for 60 seconds. Now the incredibly small tin particles have been dispersed and can do their job of opacifying the glaze. Would sieving the slurry have worked? No, the particle agglomerates can be far smaller than the openings in an 80-mesh sieve (individual particles could be 1000 times smaller!). The thorough dispersion of the expensive tin oxide particles has real benefit: It enables making an accurate assessment of whether the 5% addition is enough. In this case it isn't, more is needed.

This picture has its own page with more detail, click here to see it.
This is also a common problem at low fire on earthenware clay (but can also appear on a buff stonewares). Those white spots you see on the beetle also cover the entire glaze surface (although not visible). They are sites of gas escaping (from particles decomposing in the body). The spots likely percolate during soaking at top temperate. Some of them, notably on the almost vertical inner walls of this bowl, having not smoothed over during cool down.
What can you do? Use the highest possible bisque temperature, even cone 02 (make the glaze thixotropic so it will hang on to the denser body, see the link below about this). Adjust the glaze chemistry to melt later after gassing has finished (more zinc, less boron). Apply a thinner glaze layer (more thixotropy and lower specific gravity will enable a more even coverage with less thickness). Instead of soaking at temperature, drop 100 degrees and soak there instead (gassing is much less and the increasing viscosity of the melt overcomes the surface tension). Use a body not having any large particles that decompose (and gas) on firing. Use cones to verify the temperature your electronic controller reports.

This picture has its own page with more detail, click here to see it.
The mug on the left, #1, is a commercial brushing glaze. It is opaque enough to cover this red-burning clay body. It shows the desired effect. That depends on the fact that opaque glazes stretch thinner on the sharp edges of incised designs. If they have enough melt mobility and are applied right, the effect is amplified. This potter is attempting to mix her own DIY equivalent as a dipping glaze, adding 4% tin oxide to a transparent base glaze in #2 and zircon (a higher percentage) in #3. As you can see, the effect is not working as well, and there are several reasons:
#2 is whiter because it uses tin oxide as the opacifier (vs. zircon, likely used in #1). #2 and #3 have less melt fluidity; the base is likely G2926B. #1 was applied by brush, the others using a dipping glaze. Matching the original involves a combination of things: A base having more flux (especially B2O3) is needed (e.g. G3806C). Careful control of application thickness. The right percentage of opacifier. And, it may be necessary to mix the DIY version as a brushing glaze, that method of application might be needed to get the careful control of thickness and thickness variation needed.

This picture has its own page with more detail, click here to see it.
This is a cone 6 oxidation transparent glaze having enough flux (from a boron frit) to make it melt very well, that is why it is running and pooling. Iron oxide has been added (around 5%), producing this transparent amber effect. Darker coloration occurs where the glaze has run thicker (because it absorbs more light). This simple mechanism enables the glaze to automatically highlight contours, emboss and textures on the underlying surface. This mechanism works with any color in almost any transparent base glaze, as long as bubble clouding and crystallization do not occur. Entire lines of commercial glazes (e.g. AMACO Celadons) are based on this mechanism and potters prize it (industry doesn't like it because it is difficult to achieve consistency).
This glaze relies on high levels of K2O and Na2O to produce the brilliant gloss, however the side effect of that is crazing. These are sourced by feldspars, nepheline syenite and are high in certain frits. To achieve this effect, recipes must rely on other fluxes like boron, lithium or zinc.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. These are commonly used base glazes. The top one is a magnesia matte, next down is a calcia matte. They react very differently to these additions. Notice also the difference when titanium dioxide is applied thickly. Tin oxide fires whiter than zircon (e.g. Zircopax). Each opacifier has issues. Tin is expensive. Titanium is difficult to mix into the slurry (screening required), not as white or opaque, variations in thickness produce more difference in results and it can turn blue. Zircon is more likely to cutlery mark, twice as much is required and it amplifies the color of any iron present.

This picture has its own page with more detail, click here to see it.
The clay is a buff stoneware. The upper two samples are G2934, a magnesia matte. The bottom two are G1214Z1, a calcia matte. The base transparent versions are on the left and the ones on the right have 10% zircon opacifier added. The difference is surface character is visible.

This picture has its own page with more detail, click here to see it.
Tin oxide is a powerful opacifier, but the 5% in this Frit 3124 based Arbuckle Majolica cone 04 recipe on the left is not sufficient. Adding 10% zircon (e.g. Zircopax, Superpax) produces the one on the right. Would just using 15% zircon be better? No. More zircon means a stiffer melt and more issues with crawling (notice the small bare spots on the right edge). This could be managed by the addition of CMC gum or a higher clay content to get better adhesion and dry hardness). But another improvement would be worth trying first: Use 4% tin and 8% zircon. That should opacify enough and present fewer problems with crawling.

This picture has its own page with more detail, click here to see it.
This is G2934Y matte glaze base with opacifiers added. It has been applied to a dark-burning body to demonstrate the comparative degrees of opacity. The stain is Mason 6700 white. While it does not opacify nearly as well as tin or zircon, it does produce a smoother surface.

This picture has its own page with more detail, click here to see it.
On this M390 red clay test tile, the titanium-variegated cone 6 calcia matte glaze G1214Z1 looks excellent (rutile has a similar effect). But that appearance depends on a combination of factors: glaze chemistry, 5% titanium dioxide, the titanium grade, application thickness, the red M390 body and the PLC6DS firing schedule. The relief of the tile especially flatters it - forcing the glaze thin over high points and allowing it to pool in recesses, displaying a whole range of effects in just a few centimetres.
The tile tells you what effects a glaze is capable of; it does not necessarily tell you what the glaze will look like on ware. These mugs demonstrate that. They were fired using the C6DHSC schedule and are made from buff-burning M340 (left) and M390. The mug on the right also has a heavier, less-even application. Surprisingly, some of the thickest runs become more transparent rather than more opaque. That is a reminder that the pale, variegated character of this glaze is not simply the result of titanium acting as an opacifier; it depends heavily on melt thickness and titanium-driven crystallization during cooling.

This picture has its own page with more detail, click here to see it.
Most artists and potters want some sort of visual variegation in their glazes. The cone 6 oxidation mug on the right demonstrates several types. Opacity variation with thickness: The outer blue varies (breaks) to brown on the edges of contours where the glaze layer is thinner. Phase changes: The rutile blue color swirls within because of phase changes within the glass (zones of differing chemistry). Crystallization: The inside glaze is normally a clear amber transparent, but because these were slow cooling in the firing, iron in the glass has crystallized on the surface. Clay color: The mugs are made from a brown clay, the iron within it is bleeding into the blue and amplifying color change on thin sections.

This picture has its own page with more detail, click here to see it.
These pairs are G2934 matte and G2916F glossy cone 6 base glaze recipes. The left pair has 5% maroon stain added, the right pair 5% purple stain. Why? The Mason Colorworks reference guide has the same precaution for both stains: the host glaze must be zincless and have 6.7-8.4% CaO (this is a little unclear, it is actually expressing a minimum, the more the CaO the better). The matte recipe calculates to 11% CaO, the glossy to 9%. So there is enough CaO. The problem is MgO (it is the mechanism of the matteness in the left two), it impedes the development of both colors (although not mentioned on the Mason docs).

This picture has its own page with more detail, click here to see it.
On the left: G2571A dolomite matte fired at cone 10R. Right: 10% Zircopax has been added. Both are on a buff stoneware (H550 from Plainsman Clays).

This picture has its own page with more detail, click here to see it.
This GLFL test for melt flow demonstrates how zircon opacifies but also stiffens a glaze melt at cone 6. Zircon also hardens many glazes, even if used in smaller amounts than will opacify.

This picture has its own page with more detail, click here to see it.
This is a 45:27:28 Gerstley Borate:Kaolin:Silica base on a dark firing clay body. But tin oxide will do that in almost any cone 6 clear glaze (use one that fits your clay body).

This picture has its own page with more detail, click here to see it.
An example of how a micro-bubble population in the matrix of a transparent glaze can partially opacify it. If this glaze was completely transparent, the red clay body would show much better. However this is not the fault of the glaze. On a white body it would be more transparent. The problem is the terra cotta body. This is fired at cone 02. As the body approaches vitrification the decomposition of particles within it generate gases that bubble up in to the glaze. A positive aspect of this phenomena that this glaze could be opacified using a lower percentage of zircon.
This type of glaze responds better to opacifier additions.

This picture has its own page with more detail, click here to see it.
Left: G2934 cone 6 matte glaze with 3% Mason 6300 blue stain. Right: An additional 4% tin added. The thickness of application is close to the same. Notice how an opacified color does not have depth and therefore is lighter in color. Also it does not break to different shades at the edges of contours the way the transparent color does.

This picture has its own page with more detail, click here to see it.
A melt fluidity comparison between two cone 6 matte glazes. G2934 is an MgO saturated boron fluxed glaze that melts to the right degree, forms a good glass, has a low thermal expansion, resists leaching and does not cutlery mark. G2000 is a much-trafficked cone 6 recipe, it is fluxed by zinc to produce a surface mesh of micro-crystals that not only mattes but also opacifies the glaze. But it forms a poor glass, runs too much, cutlery marks badly, stains easily, crazes and is likely not food safe! The G2934 recipe is google-searchable and a good demonstration of how the high-MgO matte mechanism (from talc) creates a silky surface at cone 6 oxidation the same as it does at cone 10 reduction (from dolomite). However it does need a tin or zircon addition to be white.

This picture has its own page with more detail, click here to see it.
This is G2934 cone 6 matte (left) with 10% zircon (center), 4% tin oxide (right). Although the base unopacified recipe does not cutlery mark the other two do. Although the marks clean off all of the two on the right, the zircon version (in this case Zircopax) version has the worst and is difficult to clean. Thus, a small change is all that is likely needed. One solution is to reduce the matteness of this glaze, moving to more toward a satin surface. A way to do this is to line-blend in a glossy glaze to create a compromise between the most matteness possible yet a surface that does not mark or stain. Another option is to switch to 400 mesh silica in the recipe, that will enable many more of the particles to go into solution in the melt, thus increasing the gloss a little (an improving the firing surface in other ways).

This picture has its own page with more detail, click here to see it.
On Plainsman H443 iron stoneware in reduction firing. Notice Tin does not work. Also notice that between 7.5 and 10% Zircopax provides as much opacity as does 15% (Zircon is very expensive).
![]() Zircopax, tin oxide, titanium as opacifiers in four base glazes |
| Glossary |
Base Glaze
Understand your a glaze and learn how to adjust and improve it. Build others from that. We have bases for low, medium and high fire. |
| Glossary |
Variegation
Ceramic glaze variegation refers to its visual character. This is an overview of the various mechanisms to make glazes dance with color, crystals, highlights, speckles, rivulets, etc. |
| Glossary |
Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it. |
| Glossary |
Colorant
In ceramics and pottery, colorants are added to glazes as metal oxides, metal-oxide-containing raw materials or as manufactured stains. |
| Glossary |
Boron Blue
Boron blue is a glaze fault involving the crystallization of calcium borate. It can be solved using glaze chemistry. |
| Glossary |
Cutlery Marking
Ceramic glazes that mark from cutlery are either not properly melted (lack flux), melted too much (lacking SiO2 and Al2O3), or have a micro-abrasive surface that abrades metal from cutlery. |
| Glossary |
Majolica
Majolica is a tradition of Italian Renaissance white opaque glazed red earthenware having brightly colored brushwork decoration. Knowing some technical details will help you better succeed with the process. |
| Glossary |
Opacity
Opacity of ceramics glazes is normally achieved by adding an opacifier like tin oxide or zircon. However, there are chemical profiles that can turn transparent glazes milky and make it cheaper to opacify them. |
| Properties | Glaze Opacifier |
| Properties | Glaze Variegation |
| Projects | Properties |
| Materials |
Titanium Dioxide
A super white powder used in ceramic glazes to variegate, opacify and moderate color. |
| Materials |
Tin Oxide
Its principle use in ceramics is as an opacifier in glazes. It is very expensive. |
| Typecodes |
Opacifier
Opacifiers are powders that turn transparent glazes opaque by various chemical and physical mechanisms (and combinations of mechanisms). |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk