0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Opacity

Opacity of ceramics glazes is normally achieved by adding an opacifier like tin oxide or zircon. However, there are chemical profiles that can turn transparent glazes milky and make it cheaper to opacify them.

Key phrases linking here: opacity - Learn more

Details

Ceramic glaze opacity refers to the degree to which a glaze is non-transparent. Non-colored glazes can be either transparent, opaque or somewhere in between. Transparent glazes are glossy (matt glazes, by definition, are never completely transparent but they can be partly translucent to reveal underglaze decoration, for example). Opaque glazes are normally just transparent glazes with additions of light-reflecting opacifer particles (like tin oxide or zircon) that do not melt and dissolve into the glaze with the rest of the oxides. Often, significant percentages of opacifier must be added to a transparent glaze to achieve complete opacity. Tin oxide is by far the most expensive, whiteness can be achieved with 7% or less (whereas 10-20% zircon opacifier is needed to get full opacity). Zircon materials are almost always the most practical. The finer the particle size the better they opacify. It is really quite amazing that such small particles can resist being dissolved into the glaze melt, this is a testament to how refractory they really are - other common ceramic material particles do not even come close to being able to do this.

Glaze opacity can be 'designed in' and a result of crystallization that is occurring as the glaze melt cools, it can be the product of a simple addition of opacifier or it can be a combination of both, or it can be a glaze defect (e.g. incomplete melting, devitrification). Different glaze bases respond differently to opacification mechanisms and a good knowledge and testing regimen is needed to produce a good opaque glaze that is not overly expensive and does not exhibit some of the common problems associated with opacity (cutlery marking, poor glaze melt fluidity and associated issues like blistering and pinholing). Opaque glaze frits are available, the opacifier is smelted right in during the manufacturing process, these work the best not only in firing, but assure a better dispersion of the opacifier particles.

The degree of opacity of a colored glaze determines its depth of color. Transparent glazes have depth, thus any colorants present produce deep and rich color (if the glaze does not crystallize of course). Opacification subdues color by reducing its depth. Thus a deep rich blue can turn into a dull pastel blue when the glaze is opacified. Partially opacified glazes are sometimes referred to as 'milky'. People testing opacification quickly learn how many shades of white there can be (depending on opacifier used, its percentage, kiln atmosphere and impurities present). Zircon opacifiers tend toward yellower whites whereas tin oxide produces bluer ones. Unlike opacified glazes that exhibit the same color regardless of thickness, the intensity in a colored transparent varies according to thickness (twice as thick will be twice as dark).

There are a number of mechanisms of glaze opacity. These include the simple dispersion of refractory micro-particles (zircon or tin for example) that reflect and refract the light, the development of opaque crystalline phases in the glaze during cooling (from high CaO for example), the surface smoothness (mattes are often more opaque partly because the surface is not flat and scatters light), the development of multiple phases within the glaze matrix (islands of differing glass composition and structure which refract light as it passes through the borders between phases). Suspended micro-bubbles in a glaze will also scatter light and can produce a milky effect. Of course, the degree of melting will also affect the completeness to which transparency is developed.

If whiteness and homogeneity are needed (e.g. toilet bowl white), the opacification options are quite narrow, usually only tin and zircon additions are feasible. But for colored glazes, opacifiers that yellow or variegate the glaze (like titanium or rutile) are options (but more difficult to maintain). CaO and ZnO like to crystallize and can do this to the point that the entire glaze surface is covered with micro-crystals that are completely opaque.

A good example of opacity occurring when it is not wanted is boron blue. When boron is too high, especially when there is plenty of SiO2 and Al2O3, boron forms crystal phases that turn transparent glazes milky. However, since opacifiers are very expensive, this effect could be used to reduce the cost of opacification.

Colorants in transparent glazes produce the effect of varying color with varying glaze thickness. This is often a sought-after effect to highlight surface and contour variations in a piece. But on flat surfaces the phenomenon can detract from the appearance, highlighting thickness variations that occurred during application (e.g. runs).

Opacity is also critical in engobes, this is because their normal purpose is to hide the body below. Opaque engobes do not have a melting phase and can thus be completely opaque even if applied very thinly. Thus, zircon is not needed. That being said, zircon is added to them to produce the whitest possible color.

Related Information

A comparative glaze opacity test in a tile lab:

The way to minimize Zircon


This picture has its own page with more detail, click here to see it.

Strips of the same glaze recipe, each containing different percentages of zircon opacifier, have been applied across both a dark-burning body and a white engobe. While it is difficult to measure the absolute degree of opacity from a photo like this, the side-by-side comparison makes differences easy to see. Tests like this demonstrate that simple visual comparisons can often be as useful as instrument measurements when evaluating glaze opacity. Colorimeters measure Lab* color values, not opacity directly. This test is really about visual hiding power, which instruments don't always capture well.

In this case the technician may be trying to determine how to achieve the required whiteness at minimum cost. Both the engobe and glaze contain zircon. The whiter the engobe the less opacifier is required in the glaze over it. Zircon is an expensive material, and reducing the total needed by even by 1% can make a significant difference in production cost.

The same test method can also be used to compare different brands of zircon opacifier in the same recipe.

A subtle aspect can be noted by coverage on the dark body: Opacity differences there become visible, whereas on the white engobe, differences almost disappear. Where an engobe is not to be used, an effective tweak is to add a thin black line under the glaze, then the lowest zircon level that hides the line becomes obvious.

DIY the commercial glaze on mug #1:

You must consider five factors to make it work


This picture has its own page with more detail, click here to see it.

The mug on the left, #1, is a commercial brushing glaze. It is opaque enough to cover this red-burning clay body. It shows the desired effect. That depends on the fact that opaque glazes stretch thinner on the sharp edges of incised designs. If they have enough melt mobility and are applied right, the effect is amplified. This potter is attempting to mix her own DIY equivalent as a dipping glaze, adding 4% tin oxide to a transparent base glaze in #2 and zircon (a higher percentage) in #3. As you can see, the effect is not working as well, and there are several reasons:

#2 is whiter because it uses tin oxide as the opacifier (vs. zircon, likely used in #1). #2 and #3 have less melt fluidity; the base is likely G2926B. #1 was applied by brush, the others using a dipping glaze. Matching the original involves a combination of things: A base having more flux (especially B2O3) is needed (e.g. G3806C). Careful control of application thickness. The right percentage of opacifier. And, it may be necessary to mix the DIY version as a brushing glaze, that method of application might be needed to get the careful control of thickness and thickness variation needed.

The covering power and opacity of an encapsulated stain


This picture has its own page with more detail, click here to see it.

This cone 6 porcelain bowl has a black engobe inside and half way down the outside. This inside glaze is a transparent (G2926B) but the outside is that same transparent with 11% added encapsulated red stain. Notice that the glaze is so opaque that you cannot see where the black engobe ends and the while porcelain body begins!

Boron blue in low fire transparent glazes


This picture has its own page with more detail, click here to see it.

This high-boron high-CaOcone 04 glaze is generating calcium-borate crystals during cool down (called boron-blue). This is a common problem and a reason to control the boron levels in transparent glazes; use just enough to melt it well. If more melt fluidity is needed, decrease the percentage of CaO in favor of a lower melting oxide, that will certainly help. There is a positive: For opaque glazes, this effect can actually enable the use of less opacifier.

Here’s why engobes shouldn’t melt

And also why they needn't contain zircon


An over mature engobe is not opaque

This picture has its own page with more detail, click here to see it.

Since white burning slips are made from refractory materials they are not nearly as vitreous as terracotta bodies, they need help to mature and a frit is the natural answer. With the right amount, fired shrinkage can be matched to the body while the slip remains opaque.

L3685A slip on the left: An adjustment to the popular "Fish Sauce" recipe (which is basically a super plastic white body). 8% Frit 3110 replaces 8% Pyrax to make it glass-bond to the body better while remaining completely opaque.

Right L3685C: It has 15% frit, moving it into glaze territory, with translucency replacing opacity. Although expensive zircon could be added to restore opacity, that doesn’t fix the excessive firing shrinkage it now has, mismatching it with the body (which becomes more eventful the thicker it is applied).

The action of Zircopax vs Tin Oxide at cone 10R


This picture has its own page with more detail, click here to see it.

On Plainsman H443 iron stoneware in reduction firing. Notice Tin does not work. Also notice that between 7.5 and 10% Zircopax provides as much opacity as does 15% (Zircon is very expensive).

Al2O3 in glazes make them durable and wear resistant


This picture has its own page with more detail, click here to see it.

The cone 6 glazes on the left have double the boron of those on the right so they should be melting much more. But they flow less because they have much higher Al2O3 and SiO2 contents. This effect renders them milky white vs. the transparent of those on the right. Why? Because G and H are trapping micro-bubbles because of the increased viscosity of the melt. In spite of this, the two on the left do fire almost transparent when applied to ware, they have enough fluidity to shed most of the bubbles when in a thin layer. The ones on the right are too fluid, they will run excessively on ware unless applied thinly. The sweet-spot is a little more fluidity than those on the left. But there is another very important factor: Durability. The increased Al2O3 in G and H make them fire harder, more resistant to abrasion. The added SiO2 adds resistance to leaching.

Does Zircopax only whiten and opacify a clear glaze? No.


This picture has its own page with more detail, click here to see it.

This GLFL test for melt flow demonstrates how zircon opacifies but also stiffens a glaze melt at cone 6. Zircon also hardens many glazes, even if used in smaller amounts than will opacify.

Unwanted streaking in a glaze:

Uneven laydown is the likely reason


A mug with streaks of lighter blue on a darker blue background

This picture has its own page with more detail, click here to see it.

This is a fluid melt cone 6 glaze with colorant added and partially opacified. It runs into contours during firing, thickening there (notice the darkening around the logo), this is a desired visual effect. However, notice that drips and runs coming down from the rim, they are producing darker streaks. This is a laydown issue. Dipping glazes that fasten-in-place too slowly will often drain unevenly on extraction from the bucket. This can be solved by making slurries thixotropic. Even on dense bisque, they will fix-in-place in an even layer. Glazes having sufficient clay (e.g. 15% kaolin) will gel more easily (to become thixotropic). Slurries containing significant CMC gum may apply evenly but thinly (and dry slowly, with drips).

Links

Glossary Boron Blue
Boron blue is a glaze fault involving the crystallization of calcium borate. It can be solved using glaze chemistry.
Glossary Mechanism
Identifying the mechanism of a ceramic glaze recipe is the key to moving adjusting it, fixing it, reverse engineering it, even avoiding it!
Glossary Opacifier
Glaze opacity refers to the degree to which it is opaque. Opacifiers are powders added to transparent ceramic glazes to make them opaque.
Materials Zircopax
Zirconium silicate, its principle use in ceramics is as an opacifier in glazes. It is an expensive material, but less so than tin oxide.
Materials Zircon
Zircon (zirconium silicate) is a hard, dense, refractory ceramic material used to opacify pottery glazes and in refractory products such as kiln washes, crucibl

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy