0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Crystallization

Ceramic glazes form crystals on cooling if the chemistry is right and the rate of cool is slow enough to permit molecular movement to the preferred orientation.

Key phrases linking here: crystallization, devitrification, devitrify - Learn more

Details

Depending on the chemistry of a glaze melt, it may "prefer" to solidify as an organized molecular structure, or it may prefer solidifying as a glass. The determining factor is the flux ions (Ca²⁺, Na⁺, K⁺, Mg²⁺) that sit in the gaps, breaking up the silicate network. As the melt cools, the system wants to move toward a lower-energy, more ordered state. Sodium and potassium are “happy” staying dissolved in the glass. Others, like calcium or zinc, are “happier” forming specific, stable crystal lattices. Where the chemistry and cooling curve are right, crystals will grow. But if cooling is faster, they solidify as a glass.

Photo not found
or not published

Crystals can grow in cooling glaze melts if one or more of the following conditions are present: the glaze melt is fluid, cooling rate is slow, oxides that most readily form crystals are present (e.g. ZnO, TiO2), oxides that can form crystals are present in high proportions (e.g. CaO, Fe2O3), oxides that stiffen the melt are not present or present in low percentages (e.g. Al2O3, Zr particles which crowd the melt by not dissolving, and MgO at lower temperatures). Crystals are normally silicate or borate compounds. But, aluminate crystals are also possible. Nucleation most often happens at a higher temperature than growth. This is why some crystalline potters "strike" the kiln (dropping the temp quickly to stop new seeds from forming) and then "hold" at a lower temperature to allow the existing seeds to grow. Crystals can actually be "seeded" by incorporating the seeds into a glaze batch. Glazes not normally prone to crystallization can sometimes be partially crystallized by very slow cooling.

Crystallization can be highly decorative (thus sought-after by potters) but is difficult to maintain consistency (and is thus often used in one-of-a-kind art ware). Potters go to great lengths to achieve reactive glazes and crystallization is a prime mechanism. We have seen potters use glaze recipes with as much as 13% tin oxide, an incredibly expensive material - the ecstasy of the visual aesthetics giving them amnesia of the cost!

Unwanted crystallization occurring in a glaze during cool-down in the firing is called devitrification; it spoils gloss surfaces and can be a real plague in industry. There is less flexibility in cooling rate so adjustments to chemistry must be made (e.g. higher Al2O3, switching some CaO for MgO, reducing B2O3).

Very glossy or well-melted glazes can be subject to this because they likely either contain a lot of SiO2 (which combines with other oxides to form silicate crystals) or have a very fluid melt (which enables crystals greater freedom to form). When devitrification is desired, it is simply called crystallization. The chemistry of the host glaze is the key factor since it determines the amount of melting and the presence of oxides that are crystal-friendly or not. Many mattes are simply glossy glazes in which the entire surface has been invaded by micro-crystals. Decorative crystalline glazes often rely heavily on Na2​O (Soda) to achieve the necessary fluidity, but because Soda has a high CoE (Coefficient of Expansion), these glazes are notorious for crazing.

A dramatic example of crystallization can be demonstrated by melting (and cooling) a powdered mix of 50:50 Ferro frit 3134 and cobalt oxide in a crucible at cone 6. The frit is a very active melter (it contains no alumina) and the cobalt is also an active melter, together they can work real crystal magic!

Related Information

Secret #2 of crystalline glazes:

The chemistry


Close up of glaze crystals

This picture has its own page with more detail, click here to see it.

Close-up of a crystalline glaze. These crystals grow because both the glaze chemistry and the firing schedule have been tuned specifically to make that happen. The melt must be very fluid, so they contain lots of flux and very little Al2O3 (since alumina stiffens the melt and inhibits crystal growth). They also contain lots of ZnO and enough SiO2 to form zinc-silicate crystals. Since clays and feldspars contribute alumina, crystalline recipes use very little of either, relying on frits and other low-alumina materials.

This is very much DIY territory. You test, adjust, document and repeat. The best crystalline glaze people often do hundreds of firings to dial in a recipe and firing schedule.

Additions of iron oxide are coloring, fluxing and crystallizing this base transparent


Glazes range from celadon to heavy iron crystal surface

This picture has its own page with more detail, click here to see it.

Iron oxide is an amazing glaze addition in reduction. Here, I have added it to the G1947U transparent base. It produces green celadons at low percentages. Still transparent where thin, 5% produces an amber glass (and the iron reveals its fluxing power). 7% brings opacity and tiny crystals are developing. By 9% color is black where thick, at 11% where thin or thick - this is “tenmoku territory”. 13% has moved it to an iron crystal (what some would call Tenmoku Gold or Teadust), 17% is almost metallic. Past that, iron crystals are growing atop others. These samples were cooled naturally in a large reduction kiln using the C10RPL firing schedule, the crystallization mechanism would be heavier if it were cooled more slowly (or less if cooled faster). The 7% one in this lineup is quite interesting, a minimal percentage of cobalt-free black stain could likely be added to create an inexpensive and potentially non-leaching jet-black glossy.

The same glaze fires very differently depending on kiln cooling rate


This picture has its own page with more detail, click here to see it.

Both mugs use the same cone 6 oxidation high-iron (9%), high-boron, fluid melt glaze. Iron silicate crystals have completely invaded the surface of the one on the left, turning the gloss surface into a yellowy matte. Why? Multiple factors. This glaze does not contain enough iron to guarantee crystallization on cooling. When cooled quickly it fires the ultragloss near-black on the right. As cooling is slowed at some point the iron will begin to precipitate as small scattered golden crystals (sometimes called Teadust or Sparkles). As cooling slows further the number and size of these increases. Their maximum saturation is achieved on the discovery, usually by accident, of the likely narrow temperature range they form at (normally hundreds of degrees below the firing cone). Potters seek this type of glaze but industry avoids it because of difficulties with consistency.

Crystalline and vitreous silica molecular structure


This picture has its own page with more detail, click here to see it.

Several things are needed for high silica glazes to crystallize as they cool. First a sufficiently fluid melt in which molecules can be mobile enough to assume their preferred connections. Second, cooling slowly enough to give them time to do this. Third, the slow cooling needs to occur at the temperature at which this best happens. Silica is highly crystallizable, melts of pure silica must be cooled very quickly to prevent crystallization. But Al2O3, and other oxides, disrupt the silicate hexagonal structure, making the glaze more resistant to crystallization.

Thin titanium band sprayed over cone 6 glazes demonstrates crystallization


This picture has its own page with more detail, click here to see it.

The first is on GA6-A, the rest are on GA6-C (Alberta slip glazes). The last has been applied too thickly, the brown band is dry and blistered.

Reduction high temperature iron crystal glaze


This picture has its own page with more detail, click here to see it.

This is what about 10% iron and some titanium and rutile can do in a transparent base glossy glaze (e.g. G1947U) with slow cooling at cone 10R on a refined porcelain.

Cone 10R Tenmoku Ron Roy cup walks a delicate balance


This picture has its own page with more detail, click here to see it.

Each potter using Tenmoku has their own preferences about how the glaze should look. Ron clearly likes the iron crystals to develop well on the edges of contours. He has learned how to walk a delicate firing and recipe balance to achieve this effect. If the percentage of iron is too high, or the glaze is applied too thin, reduction is too heavy or the cooling too slow there will be too muchy crystallization. If the iron is too low, cooling is too fast or the glaze it too thick it will be a solid black. Additionally, this effect depends on a glaze having a fluid melt (the iron is a strong flux), if the glaze is too thick it will run downward during the firing.

An example of how cobalt can precipitate in a fluid melt glaze at cone 6


This picture has its own page with more detail, click here to see it.

This glaze has a significant amount of cobalt carbonate and during cooling the excess is precipitating out into pink crystals during cooling in the kiln. This effect is unwanted because in this case since it produces an unpleasant surface and color (the photo does not clearly show how pink it is). This problem can be fixed by a combination of cooling the kiln faster, increasing the Al2O3 content in the glaze (it stiffens the melt and prevents crystal growth) or firing lower.

Variegating effect of sprayed-on layer of titanium dioxide


Pure titanium as a varieagant

This picture has its own page with more detail, click here to see it.

The base glaze (inside and out) is GA6-D Alberta Slip glaze fired at cone 6 on a buff stoneware. However, on the outside, the dried-on glaze was over-sprayed with a very thin layer of titanium and water (VeeGum can be used to help gel the sprayable titanium slurry and suspend it). The dramatic effect is a real testament to the variegating power of TiO2. An advantage of this technique is the source: Titanium dioxide. It is a more consistent source of TiO2 than the often-troublesome rutile. Another advantage is that the variegation can be selectively applied in specific areas or as a design. This effect should work on most glossy glazes having adequate melt fluidity.

Cone 10R variegation and crystal magic


This picture has its own page with more detail, click here to see it.

This is an example of crystallization in a high MgO matte. MgO normally stiffens the glaze melt forming non-crystal mattes but at cone 10R many cool things happen with metal oxides, even at low percentages. Dolomite and talc are the key MgO sources.

Variegation and phase separation with about 5% rutile


This picture has its own page with more detail, click here to see it.

The glaze is a dolomite matte fired to cone 10R. High fire reduction is among the best processes to exploit the variegating magic of rutile.

Same glaze, same kiln, same clay: The right one crystallized. Why?


This picture has its own page with more detail, click here to see it.

Well, actually they are not exactly the same. This is 80% Alberta Slip and 20% frit. But the frit on the left is Ferro 3195 and on the right is 3134. By comparing the calculated chemistry for these two we can say that the likely reason for the difference is the Al2O3 content. Frit 3134 has almost none whereas 3195 has 12%. Al2O3 stiffens the glaze melt, that impedes crystal growth. And it stabilizes the melt against running during firing. Frit 3195 is thus much more "like a glaze" than is 3134, it is what Alberta Slip needs to melt as a transparent glass under normally cooling in the kiln.

Rutile in functional glazes:

Push the limit and you might get this


Rutile saturated glazes

This picture has its own page with more detail, click here to see it.

The 80:20 GA6-A Alberta Slip base becomes oatmeal-like when oversaturated with rutile and/or titanium (left: 6% rutile + 3% titanium dioxide; right: 4% rutile + 2% titanium dioxide). The rough surface results from excessive crystallization of titanium-bearing phases from the melt during cooling. It is unpleasant to touch, readily shows cutlery marking and is less desirable for functional surfaces. In glazes of this type, rutile additions above about 4% can become increasingly difficult to keep smooth and consistent. Crystallization, rather than phase separation, increasingly dominates the variegation mechanism.

One way of avoiding problems is staying below the tipping point, keeping the percentage as low as possible while still getting the desired variegation (of course, that will vary depending on the melt fluidity of the glaze and kiln cooling). Surprisingly, making the glaze more fluid does not necessarily solve the problem. Greater melt fluidity increases ion mobility and can actually promote crystal growth during cooling, producing an even rougher surface.

Tin oxide stops crystallization in GA6-A Alberta Slip base glaze


This picture has its own page with more detail, click here to see it.

Both of these mugs were soaked 15 minutes at cone 6 (2200F), then cooled at 100F per hour to 2100F and soaked for 30 minutes and then cooled at 200F/hour to 1500F. This firing schedule was done to eliminate glaze defects like pinholes and blisters. Normally the GA6-A glaze crystallizes (devitrifies) heavily with this type of firing, but an addition of 1% tin oxide to the one on the left has prevented this behavior.

A problem with brilliantly colored fluid-melt glazes: Micro-crystals


This picture has its own page with more detail, click here to see it.

Crystallization (also called devritrification). You can see the tiny crystals on the surface of this copper stained cone 6 glaze (G3806C). The preferred orientation of metallic oxides is crystalline. When kilns cool quickly there is simply not enough time for oxides in an average glaze to organize themselves in the preferred way and therefore crystals do not grow. But if the glaze has a fluid melt and it cools slowly through the temperature at which the crystals like to form, they will. There is another issue here also: There are tiny dimples in the surface. This is because copper carbonate was used here instead of copper oxide. During firing, it generates carbon dioxide (because it is a carbonate) that bubbles out of the melt, leaving behind dimples that may or may not heal during cooling.

Devitrification of a transparent glaze


This picture has its own page with more detail, click here to see it.

This glaze consists of micro fine silica, calcined EP kaolin, Ferro Frit 3249 MgO frit, and Ferro Frit 3134. It has been ball milled for 1, 3, and 6 hours with these same results. Notice the crystallization that is occurring. This is likely a product of the MgO in the Frit 3249. This high boron frit introduces it in a far more mobile and fluid state than would talc or dolomite and MgO is a matting agent (by virtue of the micro crystallization it can produce). The fluid melt and the fine silica further enhance the effect.

Crystallization of Rutile at cone 6 completely subdued? How?


This picture has its own page with more detail, click here to see it.

These glazes are both 80% Alberta Slip, but the one on the right employs 20% Ferro Frit 3249 accelerate the melting (whereas the left one has 20% Frit 3134). Even though Frit 3249 is higher in boron and should melt better, its high MgO stiffens the glaze melt denying the mobility needed for the crystal growth.

A cone 10R high iron glaze has run off the vase during firing. And crystallized.


An high iron glaze has melted too much run

This picture has its own page with more detail, click here to see it.

Iron, in the FeO form, is among the most powerful of fluxes in reduction firing. That fluxing action, dependent on the percentage of iron oxide in the recipe, produces two obvious consequences: Running (depending on the degree of reduction) and crystallization (depending on the speed of cooling and the chemistry of the glaze hosting the iron). This piece was slow-cooled during firing, resulting in total crystallization of the surface. The crystals are larger and densely packed at the neck. Their presence, as a thin surface layer, has completely matted it. And, because of the fluxing power of the FeO (present because of the reduction atmosphere in the kiln) enough glaze ran downward off the piece that it was left sitting in a pool of molten glass.

Why does the inside glaze crystallize with one frit and not the other?


Two glazes, two chemistries

This picture has its own page with more detail, click here to see it.

It is about the oxide chemistry, as shown calculated below the recipes in my account at insight-live.com. These glazes are fired at cone 6 using the C6DHSC schedule (we are focussing on the amber glossy glaze on the insides of the mugs). Most oxides want to form silicate crystals (combine with SiO2) as the glaze cools (if the cooling ramp is slow enough), iron oxide is not the least of these. Alumina (Al2O3) stabilizes the melt, that means it helps the melt to solidify as a glassy solid, not a crystalline one (thus, it does not devitrify). Notice the two Al2O3 values (black-on-red numbers): The glaze on the right has much less. That is because Ferro Frit 3134 contains almost no Al2O3 (notice in the blue panel, only 2%). The alumina in the glaze on the left, sourced more abundantly by Frit 3195, readily releases in the melt, ready to take on its job: Stiffen it and impede the formation of iron silicate crystals during cooling to create a better glass.

Crystallization of this glaze gives insight into why it can host the floating blue effect


Crystallization of a floating blue base

This picture has its own page with more detail, click here to see it.

These two mugs have the Alberta Slip base cone 6 GA6-A glaze on the inside and GA6-C on the outside (it just adds rutile to GA6-A). The left one was cooled normally (kiln off at cone 6 after soak). For the mug on the right, the kiln was soaked for half an hour at 1800F on the way down to develop the rutile blue glaze on the outside. But during this period crystallization occurred on the inside also. This provides an insight into my this GA6-A base hosts floating blue effects but GA6-B does not: The amount of Al2O3 is much lower, that improves melt fluidity and acts as a catalyst for crystallization.

Alberta Slip GA6-A glaze slow-cooled goes matte


GA6-A sow cooled

This picture has its own page with more detail, click here to see it.

This is GA6-A Alberta Slip base glaze (80 Alberta Slip:20 Frit 3134) fired using the C6DHSC firing schedule (on Plainsman M390 iron red clay). If this is cooled rapidly or 1% tin oxide inhibitor is added, it fires to a glossy clear amber glass with no crystals. This base is needed to make GA6-C rutile blue; otherwise I recommend the GA6-B base (which uses frit 3195 instead), it has a lower thermal expansion and guarantees gloss regardless of cooling speed. If, on the other hand, you want to enhance this effect, just add a little more frit (to gloss it more) and more iron oxide (that should enable matting even at faster cooling speeds.

Inbound Photo Links



An iron crystal glaze on a buff stoneware at cone 10R

Links

Glossary Glass vs. Crystalline
In ceramics, understanding the difference between what a glass and crystal are provides the basis for understanding the physical presence of glazes and clay bodies.
Glossary Vitrification
A process that happens in a kiln, the heat and atmosphere mature and develop the clay body until it reaches a density sufficient to impart the level of strength and durability required for the intended purpose. Most often this state is reached near zero p
Glossary Amorphous
Glossary Base Glaze
Understand your a glaze and learn how to adjust and improve it. Build others from that. We have bases for low, medium and high fire.
Glossary Boron Blue
Boron blue is a glaze fault involving the crystallization of calcium borate. It can be solved using glaze chemistry.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Crystalline glazes
A type of ceramic glaze made by potters. Giant multicolored crystals are grown on a super gloss low alumina high zinc glaze by controlling multiple holds and soaks during cooling in the kiln.
Glossary Matte Glaze
Random material mixes that melt well overwhelmingly want to be glossy, creating a matte glaze that is also functional is not an easy task.
Properties Glaze Crystallization
Properties Glaze Variegation

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy