EP Kaolin

Alternate Names: EPK, Edgar Plastic Kaolin, EPK Kaolin

Description: Plastic White Firing Kaolin

Oxide Analysis Formula Tolerance
CaO 0.18% 0.01
K2O 0.33% 0.01
MgO 0.10% 0.01
Na2O 0.06% -
TiO2 0.37% 0.01
Al2O3 37.36% 1.00
P2O5 0.24% -
SiO2 45.73% 2.08
Fe2O3 0.79% 0.01
LOI 13.20%n/a
H2O 1.40%n/a
SO3 0.21%n/a
Oxide Weight 232.50
Formula Weight 272.92

Notes

If you have issues getting this there are alternatives. If EPK is being used in a glaze and the percentage is low (e.g. 10-20%) switching to another will likely have minimal effect on fired properties. However, slurry properties might change. EPK helped dipping glaze slurries to gel, making them thixotropic. It was also sticky. Both Grolleg and New Zealand kaolin impart similar properties. Up to about 25% could be tolerated in glazes before drying cracks became an issue. Pioneer kaolin didn’t gel but plasticity was about the same. #6 Tile kaolin is far more plastic and, like Pioneer, but isn’t thixotropic, 20% may be the maximum to avoid drying cracks (if more kaolin is needed or there are other plastics in the recipe, e.g. Gerstley Borate, then a mix of calcined and raw kaolin can be tuned to produce the right balance of suspension and dry hardness with good drying).

In porcelains, EPK fires whiter than most other North American kaolins. The fired whiteness, reasonable plasticity and competitive pricing were valued by clay body manufacturers. If whiteness is important consider substituting New Zealand or Grolleg kaolins. Switching for Grolleg will improve body whiteness somewhat. Depending on the percentage, New Zealand kaolin could make the body fire much whiter. Of course, these two kaolins are much more expensive. A practical approach is to substitute whichever kaolin you have and assess fired color and plasticity. If plasticity is lost just add a the amount of bentonite needed to restore it (e.g. 1-3%). If body workability is most important then #6 Tile kaolin is the right choice, it is the most plastic North American kaolin (actually, it might increase plasticity so much that the percentage of bentonite can be dropped).

In review: EPK is a secondary water-washed kaolin mined in Florida, USA. EPK, when wet, is sticky and thixotropic, for these reasons it is considered by many to be the best North American kaolin for use in suspending ceramic glazes. 15-20% will normally make the glaze gel slightly, thus when a piece is immersed in the slurry and removed it drips very little and the wet glaze layer stays in place for the time it takes to dewater. And it dries relatively hard. Since EPK is close to theoretical kaolin chemistry, it will substitute for any other such kaolins chemically (but not necessarily phyically). If the percentage is greater than 25% consider splitting it with calcined kaolin to prevent crawling.

EPK is whiter burning than other American kaolins, this is due to its relatively low iron content, but more importantly the low level of TiO2: 0.4 TiO2. While this is high compared to Grolleg and Super Standard Porcelain kaolins (about 0.05%), but other common American kaolins have multiple times more TiO2 than EPK!

EPK has excellent casting properties. But it is not plastic enough for throwing bodies, it must be augmented by a more plastic kaolin (like 6Tile) or by a plasticizer like bentonite, smectite or hectorite. Or, if whiteness can be sacrificed, by a ball clay.

This material is mined and processed in Edgar Florida. It is extracted hydraulically (a high-pressure stream of water is used to wash the clay/sand mix from the bank into a small lake). The slurry is pumped and transported to vibrating screens that separate out the sand and grade it into sizes. The clay that passes the screens is pumped into a pond and settled with the aid of a flocculant. The slurry is then dried and the flocculant neutralized. The main product at the mine is high-quality white sand, the clay is a byproduct. The company is confident that there are reserves for the next hundred years.

Related Information

What made EP Kaolin unique?

What can be substituted?


EPK kaolin slurry gels

This picture has its own page with more detail, click here to see it.

In ceramics, EPK, or EP Kaolin, is used in clay bodies and glazes. EPK feels fairly plastic on wedging. But it splits like this during throwing (top right). It needs the help of bentonite or ball clay to be usable in porcelain or stoneware bodies. Tile #6 kaolin is thus a much better choice for plasticity (although higher in iron and titania).

But EPK shines in glazes. A slurry of pure EPK (bottom), mixed to only 1.15 specific gravity, holds this spatula upright! Glazes employing as little as 20% EPK, without added electrolytes, are naturally thixotropic. And its sticky nature helps with adherence and dry hardness. Consider the engobe employing it (top left). It gels and clings to this rubber spatula in an even layer, with no drips. If leather-hard ware is carefully dipped and extracted, it stays put (even if it takes hours to dry). The performance of EPK suspending glazes for use on bisque is even better.

Are there other sticky kaolins that gel? Yes. Grolleg and New Zealand kaolin. What if you cannot get either? Tile #6 is a good choice because it dries hard. But, it may need the help of Epsom Salts to produce a slurry having thixotropy like EPK.

EPK fired test bars, data, certificate and the data


Results of EPK testing

This picture has its own page with more detail, click here to see it.

All of the test bars have been fired in this project to characterize a shipment of EPK (from cone 7-10 and 10R bottom to top). The dry and fired lengths and the dry and fired weights testdata were measured and entered into an Insight-live account. The results are shown in the red-titled columns (the drying shrinkage, firing shrinkage, absorption). The weights from the sieve analysis are also shown. The calculation of water content of the plastic material (a very high 33.4%) and LOI (14.5%). I also like to take and upload a photo of the oversize material from the sieve analyses (to compare with past shipments) and of their manufacturer's certificate of analysis.

Notice the data that the manufacturer considers important to include on the certificate that they send with the shipment: Particle size, particle surface area and moisture content. Of course, they would not be able to do all the tests I do. But the product is affected by the properties of the material, so I have to test.

#6 Tile Kaolin 2021 vs EP Kaolin 2020:

Fired properties tell an unexpected story


EP Kaolin fired test bars

This picture has its own page with more detail, click here to see it.

These test bars are fired at cone 10 reduction (top) and 10, 9 and 8 oxidation (downward) - they demonstrate the importance of measuring physical properties. The charts for each show data for drying shrinkage, firing shrinkage and porosity (water absorption). The left bars are #6 Tile kaolin and the right are EPK. These two kaolins had almost the same drying shrinkages in this SHAB test, which suggests the same plasticity. And the EPK fires whiter. So it should make a better plastic porcelain, right? Not so. In reality, #6 Tile kaolin is far more plastic - EPK requires the addition of significant bentonite to equal it (bentonite is dirty and that compromises whiteness). And EPK fires less vitreous - when feldspar is added color darkens. And, although both have extremely high firing shrinkages, the EPK is much higher than the #6 Tile (even though it is not as vitreous). Bottom line: #6 Tile is a better kaolin for clay bodies.

Two batches of EP Kaolin tested quite differently in 2018


Two different batches of EPK

This picture has its own page with more detail, click here to see it.

The EP kaolin has been mixed 70:30 with nepheline syenite. This creates a body that matures below cone 6. And it enables comparing the degree to which the two kaolins influence vitrification (and their contribution to fired color in a vitreous body). The darker one is more plastic, has higher drying shrinkage more soluble salts. These dry test bars were fired at cone 4-8 and had similar fired shrinkages and porosities. However, the one on the right fired whiter at all temperatures. These differences would impact the plasticity and drying shrinkage of bodies containing a significant percentage of the material. They would also influence the ability of this kaolin to suspend slurries.

EPK fired bar (top) vs Grolleg kaolin at cone 10R. Why shrinking more?


This picture has its own page with more detail, click here to see it.

From these SHAB test bars EP kaolin appears to have a much higher fired shrinkage. But half of that happened during drying. Still, EPK shrinks 4% more during firing. Yet Grolleg produces more vitrified porcelains. The EPK bar also appears to be whiter. Yet in a porcelain body, Grolleg fires whiter. That higher drying shrinkage proves that EPK is much more plastic, right? Not really. Throwing porcelains containing either require plasticity augmentation using similar percentages of bentonite. What do we learn? To compare materials like this we need to see them "playing on the team", in a recipe working with other materials. Don't rely on material data sheets, do the testing in your recipes.

A 70:30 mix of EPK:Nepheline Syenite has gone to mush


This picture has its own page with more detail, click here to see it.

This was plastic and moldable two days ago, now it is incredibly sticky. It is being compared with 5 other kaolin:nepheline mixes, none of them have reacted in this way. The material is sourced from two mines, the other mine does not do this.

Two kaolins with different drying performance:

One always cracks, the other does not. Why?


This picture has its own page with more detail, click here to see it.

Both of these bodies are 70:30 kaolin:feldspar. The kaolin on the left (Tile #6) contains finer particles and some natural bentonitic material, giving it higher plasticity and better ability to absorb drying stresses. The EPK on the right is coarser and has less ability to redistribute stress. As the mugs dry, circumferential stresses develop near the base. The body cannot stretch enough to accommodate them, so cracks form around the bottom (or, as happens here, leave residual stresses that reveal later in bisque firing). The Tile #6 body, having greater “stress-relief plasticity”, can tolerate the strain and dries without cracking.

Is it true that during forming, the larger kaolin particles line up concentrically to the center, producing more shrinkage along radius lines than along tangents? Not likely. Clay platelets do orient during forming, but the orientation tends to be parallel to the forming surface, not radially oriented toward the center. Further, shrinkage alone does not predict cracking; uneven shrinkage does. Despite efforts to prevent it, we could not eliminate it.

While these specific cracks appear during our bisque firing, as noted, the cause originates earlier during drying. Uneven shrinkage creates residual tensile stresses in the clay. While the dried ware may appear sound, the body weakens during early firing when organic materials burn out and particle bonds weaken, releasing the stored stresses as the circumferential crack.

Thrown pieces made from pure Grolleg and EP kaolins

This is how you compare plasticities


Mugs thrown from two pure kaolins

This picture has its own page with more detail, click here to see it.

These have just been thrown on the wheel. I find it to be a foolproof method of comparing the plasticity of two clays. They were slurried up and dewatered to about the same moisture content and the same amount was thrown to compare the size achievable. While the Grolleg is stickier and dewaters a little slower, it is not nearly as plastic as EPK (which itself is not that plastic compared to others). Curiously, New Zealand kaolin (halloysite) is quite a bit less plastic than the Grolleg but it responds to plasticity augmentation (in porcelain recipes) just as well as Grolleg (similar amounts of bentonite producing similar plasticities). And, bodies containing EPK also need about the same amount of bentonite to produce plasticity suitable for throwing large forms. So, the plasticity that a kaolin appears to have by itself is not completely indicative of what it will contribute to a body (if augmented with bentonite). The EPK used here is the darker and more plastic of the two varieties Plainsman receives.

An effective test to judge the plasticity of a shipment of EP Kaolin


Throwing EPK

This picture has its own page with more detail, click here to see it.

This shipment of light EPK (there are two versions, light and dark) is just barely plastic enough to make this cylinder with a slight belly. Notice the splits on the rim, these are indicative of the shortness (low plasticity). The cohesiveness of the material, as much as plasticity, gives it a toughness to survive the stresses of throwing (an unique aspect of EPK).

Links

Minerals Kaolinite
The most fundamental clay mineral. This mineral is found in nature in its purest form as kaolin. How
Projects Testing a New Load of EP Kaolin
Kaolins can vary in many ways. Yet they are the foundation of all porcelain and light stoneware clay body recipes. It is vital to test each incoming shipment of material. Problematic brands can even require some testing on every pallet.
Glossary Thixotropy
Thixotropy is a property of ceramic slurries of high water content. Thixotropic suspensions flow when moving but gel after sitting (for a few moments more depending on application). This phenomenon is helpful in getting even, drip-free glaze coverage.
Materials Tile #6 Kaolin
The most plastic kaolin commonly available in North America, most suitable for making plastic porcelains.
Materials Edgar Glass Sand
Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Materials Pioneer Kaolin
Troubles Glaze Slurry is Difficult to Use or Settling
Understanding glaze slurry rheology is the key to solving problems and creating a suspension that does not settle out, applies well, dries crack free.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

Data

Pyrometric Cone Equivalent 35

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy