How do you make porcelain? There is a surprisingly simple logic to formulating them and to adjusting their working, drying, glazing and firing properties for different purposes.
Key phrases linking here: mullite porcelains, mullite porcelain, porcelain - Learn more
Photo not found
or not published
Photo not found
or not published

This picture has its own page with more detail, click here to see it.
Typical pottery porcelains are variations on the traditional triaxial body and commonly contain around 50% clay, either kaolin, ball clay or a mixture. Since the clay fraction is normally the largest source of iron and titanium impurities, its purity has a major influence on fired whiteness—especially in reduction.
These mugs were fired in the same kiln load at cone 10R and have the same clear glaze, G1947U. The mug on the left is a Grolleg kaolin porcelain (50% Grolleg kaolin, 25% silica and 20% Mahavir feldspar, 5% bentonite). The one on the right is 15% M23 ball clay, 40% #6 Tile kaolin, 15% Nepheline, 25% silica, 3% bentonite. The grey is the cumulative effect of the impurities in these clays.
Grolleg is considerably more expensive, but this is one place where the extra purity is plainly visible. Want to push whiteness even further? Use an ultra-low-iron New Zealand kaolin and replace ordinary bentonite with Veegum or another clean-burning plasticizer.

This picture has its own page with more detail, click here to see it.
Porcelains look much more glassy and melted than you might expect when viewed close up (this is cone 6 Polar Ice from Planisman Clays). The development of the glassy phase within the body creates a very good bond with the glaze. Actually it is a bonding zone where the glaze has melted into the body enough to create a transition rather than just a point of contact. The degree to which this transition develops determines the integrity of the bond. Of course, with porcelains it is far better developed than with stonewares and terra cottas.

This picture has its own page with more detail, click here to see it.
This body is 70:30 kaolin:feldspar (fired at cone 6 with glaze G2926B). The fired body has a vitreous porcelain-like surface. But, this dense craze pattern indicates a very serious fit problem. The COE (thermal expansion) of this body is much too low, primarily because there is no residual quartz. There isn't a glaze-fix solution to this. Reformulating it enough to fit, while maintaining the firing characteristics, would be well beyond the expertise, material availability and budget of any typical pottery or manufacturer. All that work would just boil down to "compensating for an unusually low-expansion body". Adding quartz to the body to raise its COE is the appropriate conventional solution. An initial test would be to substitute 25 of the kaolin for 200 mesh silica. It is refractory, and while the finer particles will be dissolved by the feldspar, enough of the larger pure quartz ones will remain to impose their very high COE on the fired matrix.
The other issue is with the flat particle shape of kaolin. The throwing process has lined up the predominant kaolin particles concentric to the centre. During drying, and especially firing, more shrinkage occurs across them than along them. All ten of the cups, which I made and dried in my normal, careful fashion, cracked like this! The solution is adding a filler, one with non-platy particles. Silica is perfect; the grains act like aggregate in concrete, strengthening the matrix and separating the clay particles, forcing them to orient more randomly.

This picture has its own page with more detail, click here to see it.
These are porosity and fired shrinlage test bars, code numbered to have their data recorded in our group account at Insight-live.com. Plainsman P580 (top) has 35% ball clay and 17% American kaolin. H570 (below it) has 10% ball clay and 45% kaolin, so it burns whiter (but has a higher fired shrinkage). P700 (third down) has 50% Grolleg kaolin and no ball clay, it is the whitest and has even more fired shrinkage. Crysanthos porcelain (bottom, from China) also only employs kaolin, but at a much lower percentage, thus is has almost no plasticity (suitable for machine forming only). Do H570 and P700 sacrifice plasticity to be whiter? No, with added bentonite they have better plasticity than P580. Could that bottom one be super-charged? Yes, 3-4% VeeGum or Bentone (smectite, hectorite) would make it the most plastic of all of these (at a high cost of course).

This picture has its own page with more detail, click here to see it.
Left: A porcelain that is plasticized using only ball clays (Spinx Gleason and Old Hickory #5). Right: Only kaolin (in this case Grolleg). Kaolins are much less plastic so bentonite (e.g. 2-5%) is typically needed to get good plasticity. The color can be alot whiter using a clean kaolin, but there are down sides. Kaolins have double the LOI of ball clays, so there are more gasses that potentially need to bubble up through the glaze (ball clay porcelains can produce brilliantly glassy and clean results in transparent glazes even at fast fire, while pure kaolins can produce tiny dimples in the glaze surface if firings are not soaked long enough). Kaolins plasticized by bentonite often do not dry as well as ball clays even though the drying shrinkage is usually less. Strangely, even though ball clays are so much harder and stronger in the dry state, a porcelain made using only ball clays often still needs some bentonite. If you do not need the very whitest result, it seems that a hibrid using both is still the best general purpose, low cost answer.

This picture has its own page with more detail, click here to see it.
These cone 6 clear-glazed porcelains demonstrate just how white you can make a porcelain if you use white burning kaolins and bentonites instead of ball clays. Both contain about 40% clay. The one on the left employs New Zealand kaolin and Veegum plasticizer, the one on the right Kentucky ball clays (among the whitest of ball clays in North America) and standard bentonite. Both are zero porosity. The glaze surface is a little more flawless on the right one (possibly because ball clays have a lower LOI than kaolins).

This picture has its own page with more detail, click here to see it.
Typical porcelains are made using clay (for workability), feldspar (for fired maturity) and silica (for structural integrity and glaze fit). These cone 6 test bars demonstrate the fired color difference between using kaolin (top) and ball clay (bottom). The top one employs #6 Tile super plastic kaolin, but even with this it still needs a 3% bentonite addition for plasticity. The bottom one uses Old Hickory #5 and M23, these are very clean ball clays but still nowhere near the whiteness of kaolins. Plus, 1% bentonite was still needed to get adequate plasticity for throwing. Which is better? For workability and drying, the bottom one is much better. For fired appearance, the top one.

This picture has its own page with more detail, click here to see it.
The cone 6 porcelain on the left uses Grolleg kaolin, the right uses Tile #6 kaolin. The Grolleg body needs 5-10% less feldspar to vitrify it to zero porosity. It thus contains more kaolin, yet it fires significantly whiter. Theoretically this seems simple. Tile #6 contains alot more iron than Grolleg. Wrong! According to the data sheets, Grolleg has the more iron of the two. Why does it always fire whiter? I actually do not know. But the point is, do not rely totally on numbers on data sheets, do the testing yourself.

This picture has its own page with more detail, click here to see it.
These are made from Plainsman Polar Ice translucent NZ porcelain. The one on the right was used in the coffee room of the plant and washed between uses in a common manner (which is: not very much!). The stains are obviously not nearly as visible on a stoneware mug.

This picture has its own page with more detail, click here to see it.
On the right is a porcelain used in China, renowned for its whiteness and translucency. On the left is a body made from Grolleg kaolin, this is commonly used by potters. They were fired in reduction. The tiny iron specks that potters do not even notice are enemy number for the blue-white porcelain like this. Although they might be small the reduction atmosphere makes them blossom out in full glory to ruin the piece. These specks come as contaminants in the materials (especially the silica) and they are easily picked up during fabrication. For very white bodies like this, it is incredibly difficult to prevent the specks. For a perfectly white flawless result, the entire factory must be dedicated to this one body; they use wet processing, magnets, filter pressing, stainless steel equipment and impeccable procedures.

This picture has its own page with more detail, click here to see it.
These clear glazed porcelain mugs are fired at cone 6. The one on the right has 0.2% Mason 6336 stain added to to G2926B base glaze. It matters which stain, some agglomerate and causes specking, this one disperses well.

This picture has its own page with more detail, click here to see it.
Why the difference? The one on the right (Plainsman M370) is made from commodity American kaolins, ball clays, feldspars and bentonite. It looks pretty white-firing until you put it beside the Polar Ice on the left (made from NZ kaolin, VeeGum plasticizer and Nepheline Syenite as the flux). These are extremely low iron content materials. M370 contains low iron compared to a stoneware (less than 0.5%) that iron interacts with this glaze to really bring out the color (although it is a little thicker application that comes nowhere near explaining this huge difference). Many glazes do not look good on super-white porcelains for this reason.

This picture has its own page with more detail, click here to see it.
These two unglazed porcelain tiles appear to have a similar degree of vitrification, but do they? I have stained both with a black marker pen and then cleaned it off using acetone. Clearly the one on the right has removed better, that means the surface is more dense, it is more vitreous. In industry (e.g. porcelain insulators) it is common to observe the depth of penetration of dye or ink into the matrix as an indication of fired maturity.

This picture has its own page with more detail, click here to see it.
The recipe: 50% New Zealand kaolin, 21% G200 Feldspar, 25% silica and 3% VeeGum (for cone 10R). These are the cleanest materials available. Yet it contains 0.15% iron (mainly from the 0.25% in the New Zealand kaolin, the VeeGum chemistry is not known, I am assuming it contributes zero iron). A 50 lb a box of pugged would contain about 18,000 grams of dry clay (assuming 20% water). 0.15% of 18,000 is the 27 grams of iron you see here! Even more surprising: This mug is a typical Grolleg-based porcelain using 5% of a standard iron-bearing raw bentonite. A box of it contains four times as much iron. Enough to fill that cup half full!

This picture has its own page with more detail, click here to see it.
This porcelain becomes quite brittle as it gets stiffer making it difficult to make these cuts in the foot ring. This creates extra sponging work when it is dry. It also means that dry strength will be low. Porcelains do not need to be this way, plenty of white burning bentonites are available (although they increase cost).

This picture has its own page with more detail, click here to see it.
The top Zero3 porcelain bar has 0.07% Mason 6336 blue stain added (vs. none in the bottom bar). Zero3 is a frit-fluxed body, these SHAB test bars are fired at cone 03 in oxidation. To match the color of a cone 10 reduction clear glazed Grolleg porcelain (e.g. L3778D) I add 0.05% stain blue stain (because the transparent glaze amplifies the color). In either case, to ensure that color develops, the body still must have adequate glass development (which is no problem in a fritware body).

This picture has its own page with more detail, click here to see it.
These Zero3 fritware bars are fired at cone 06, 04, 03 and 02 oxidation (bottom to top). This body has very low TiO2 and Fe2O3 levels. But the secret is the 0.2% blue stain (Mason 6336) it contains. Notice that almost no color develops at the lowest temperature, cone 06. But, as soon as glass development begins, by cone 04, so does the color.
This strategy is typically only suitable if a high-energy mixer is available. As a potter, blender mixing is thus essential to break up the stain agglomerates, otherwise tiny blue specks will appear. That mixing also separates the Veegum particles to get higher plasticity. The stain used here is Mason 6336. But this one may not work for you, just do testing to find the right one, at the right percentage.

This picture has its own page with more detail, click here to see it.
On the top you can see the color difference. The other porcelain is made from a low TiO2 mix of typical North American kaolins, feldspars and bentonites. Bottom with a light inside: Polar ice on the left is far more translucent. Yet it is not overly mature, it resists fired warping remarkably well. And it is also more plastic (which seems impossible). There is a secret to the translucency that goes beyond the fact that it employs New Zealand kaolin and the percentage of feldspar it has. But I cannot tell you. But if you read this site carefully you will discover it in the most unlikely place!
![]() Why mid-fire Grolleg porcelain is ideal for both throwing and casting |
Produced by Gemini, combining a picture of a mug I made with a generated bone china one. AI PolicyMullite and anorthite porcelains: The microstructure was only understood recently |
![]() Reduction and oxidation porcelains |
| URLs |
https://www.instagram.com/reel/DWwb-axDojA
Jingdezhen, the porcelain capital of China. Everyone works in the porcelain industry in some capacity. |
| URLs |
https://en.wikipedia.org/wiki/Jingdezhen_porcelain
Jingdezhen Porcelain at Wikipedia Porcelain made in China using the petuntse (porcelain stone) material. |
| Media |
A 3-minute Mug with Plainsman Polar Ice
Tony Hansen takes you through the steps from opening the box and wedging the clay to taking the fired mug from the kiln. |
| Glossary |
Body glaze Interface
In ceramics, the zone of adherence between glaze to the underlying body is called the clay-glaze interface. The integrity of this interface is important to strength and functionality. |
| Glossary |
Maturity
A term used in ceramics to signify the degree of vitrification in a fired clay. Mature clays are dense and strong; immature ones are porous and weak. |
| Glossary |
Stoneware
To potters, stonewares are simply high temperature, non-white bodies fired to sufficient density to make functional ware that is strong and durable. |
| Glossary |
Vitreous
The fired state of a ceramic when sufficient heat in the kiln has produced the density and strength common, and expected, in stonewares and porcelains. |
| Glossary |
Earthenware
What is the difference between earthenware and a regular stoneware body? Earthenwares lack the glass development to fill voids and glue particles. |
| Glossary |
Vitrification
A process that happens in a kiln, the heat and atmosphere mature and develop the clay body until it reaches a density sufficient to impart the level of strength and durability required for the intended purpose. Most often this state is reached near zero p |
| Glossary |
Translucency
A highly sought-after property in porcelain, fired close enough to melting to take on the glass-like property of passing light. Translucency implies tendency to warp during firing. |
| Glossary |
Clay
What is clay? How is it different than dirt? For ceramics, the answer lies on the microscopic level with the particle shape, size and how the surfaces interact with water. |
| Glossary |
Plasticity
Plasticity (in ceramics) is a property exhibited by soft clay. Force exerted effects a change in shape and the clay exhibits no tendency to return to the old shape. Elasticity is the opposite. |
| Tests |
Shrinkage/Absorption Test
SHAB Shrinkage and absorption test procedure for plastic clay bodies and materials |
| Recipes |
L2000 - 25 Porcelain
Base 25x4 porcelain recipe |
| Minerals |
Smectite
A highly plastic clay mineral related to montmorillonite (bentonite), more correctly, the name of th |
| Articles |
Formulating a Porcelain
The principles behind formulating a porcelain are quite simple. You just need to know the purpose of each material, a starting recipe and a testing regimen. |
| Materials |
Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries. |
| Materials |
Bentonite
Bentonite can make a clay body instantly plastic, only 2-3% can have a big effect. It also suspends slurries so they don't settle out and slows down drying. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk