0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Liner Glaze

Liner-glazing is a way to assure that your ware has a durable and leach resistant surface. It also signals to customers that you care about this.

Key phrases linking here: liner-glazed, liner glaze - Learn more

Details

The term "liner glaze" refers to two things. First, it is a technique (links below), where the inside and outside of a piece have different glazes that meet at the rim. Second, it refers to the practice of choosing a glaze for the inside food surfaces of utilitarian ware based more on its durability and resistance to leaching, running, crawling, blistering and crazing (problems common with reactive glazes). Glossy whites, transparents or modestly colored glazes are most common as liners. Liner glazes can have other practical purposes also. An example is their use in combination with intensely colored or variegated glazes, such are often runny and form a lake in the bottoms of vessels - this can lead to glaze compression failure.

Considerable efforts are required to produce a white or glossy glaze whose fired surface is durable to wear and tear and resistant to leaching and yet works well in the production process. Colored and reactive glazes usually hide imperfections very well, but a transparent glaze makes crazing, micro-bubbles in the matrix, clouding, boron blue, tiny surface dimples and other imperfections plainly visible. Liner glazes can also be colored (if they are well-tested and demonstrably non-leaching). Amber glazes, for example, make more visually appealing liners for dark-burning clay bodies. Colored and opacified liners also hide some imperfections better, this is important if the clay is less processed.

Liner glazes often need to be paired with specific clay bodies (or a family of bodies), primarily because different bodies have different thermal expansions (this is especially so the lower the temperature). Sometimes, the same glaze will work on different bodies, but one or more require a specific firing schedule. The liner should be thermal stress tested to be sure it will stay uncrazed over time (the 300F:Ice-water test for crazing, the Ice-water-to-boiling-water to test shivering).

Matte glazes can also be used as liners, but special effort and expertise are needed to produce a matte surface that is still silky enough to resist cutlery marking and staining. This is easiest to do at higher temperatures. Mattes produced using MgO as a mechanism are the most common.

Liner glazes are used in large quantities and need to have a slurry that stays in suspension. They need to apply to the ware in a smooth even coat, dry quickly and be durable to handling. Until now, in small industry, pottery and hobby pottery circles, clay body manufacturers have left it up to users to formulate their own liner glazes. But increasingly, users are realizing that manufacturers should take on the responsibility to supply reasonably priced pre-mixed powdered/liquid liner glazes for each of their clay bodies (or at least recommend recipes and firing schedules).

Another reason why liner glazes are simple common sense is that you can more easily see when a cup needs to be washed. In addition, although a piece might not be crazed out of the kiln, if crazing happens over time, it is easier to see this glaze in a white or transparent.

Please read the "Base Glaze" glossary page for examples of base glazes for each temperature range.

Liner glazes can be applied in such a way that they meet the outer glaze at the rim (the technique to do this is described in a separate article). Denby Pottery is a company quite skilled at doing this.

Related Information

Meet two glazes at the rim using wax emulsion. Why? How?


Liner glazed mug

This picture has its own page with more detail, click here to see it.

Reactive glazes (melt-mobile, crystallizing or heavily pigmented) are the least suitable for food surfaces because they have the potential to leach metals. Liner glazing ware is an excellent way to deal with this problem. Not only does this approach improve functionality but it can be aesthetically pleasing and practical in production.

This liner is GA6-B, a pottery glaze recipe we promote with confidence. Not only is it less likely to be leaching metals but also less likely to craze - this assures water tightness on non-vitreous bodies and eliminates any potential for bacteria growth in the cracks (especially if the body has porosity). Unfortunately, glazes that leach are also likely to stain and cutlery mark - these add more reasons why they are most often unsuitable for food surfaces.

The straightness of the dividing line is affected by both the application technique and the degree to which the two glazes bleed into each other and run. Read and watch our liner glazing step-by-step and liner glazing video for details on how to do this - it is practical for any potter or hobbyist (or even in production). And tap/click the picture above for other examples of this.

Commercial supposedly-safe glazes leaching. A liner glaze is needed.


Leaching commercial pottery glaze

This picture has its own page with more detail, click here to see it.

Three cone 6 commercial bottled glazes were layered inside this mug, which was then filled with lemon juice overnight. The whitened, altered areas show that the glaze surface has been attacked by the acid. Even if glaze A, B and C have each passed a fired-surface release test individually, A-over-B-over-C is a new fired glass composition and microstructure. The individual certifications do not logically constitute a test of that combination. The color change suggests attack on cobalt-bearing glass, but exactly what is leaching cannot be known without testing because the recipes are proprietary. For functional ware, it is better to use a stable transparent or white liner glaze whose recipe and limits are known.

When manufacturers say their products conform to standards such as ASTM D-4236, they are referring to the safety labeling of the liquid art material for the user of the product, not guaranteeing that layered fired surfaces on finished ware will be leach-resistant

Zircopax makes the liner glaze much whiter on this porcelain


This picture has its own page with more detail, click here to see it.

Although this is a whiteware body (Plainsman M370), under the transparent liner glaze (G2926B) the color appears ivory, off-white. But with 8% added Zircopax the quality of the color is transformed into a white that is even better than what a much more expensive New Zealand or Grolleg kaolin porcelain would exhibit with a transparent cover glaze. The outer glaze is G2934Y matte with a yellow stain. The glazes were applied inside and outside by pouring and dipping (it would not be possible to apply the yellow evenly enough by brushing).

Three cone 10R mugs that have the same liner glaze.


This picture has its own page with more detail, click here to see it.

The liner is G2571A dolomite matte.

Liner glaze is coffee-staining and leaching after two years. Is it toxic?


The white inside of a mug is coffee-staining

This picture has its own page with more detail, click here to see it.

This is a cone 04 terra cotta piece. The coffee stain cannot be removed because the coffee has also leached off the surface gloss. Glazes are glass. Glass is leachable if the chemistry is out-of-balance. So is this glaze poisoning the user? No, it has an insurance policy. It is transparent, made from a mix of two frits (Ferro 3124, 3134) plus kaolin and silica. The recipe contains no heavy metal colorants or pigments and no toxic fluxes like lithium or barium. But the body is red, how can the glaze be white? A white porcelain-like engobe layer was applied at the leather hard stage and it was clear-glazed after bisque. The fix: The predominant frit, 3134, has almost no Al2O3 (the oxide most important in producing durability). So I increased the Al2O3 (doing the chemistry in my Insight-live.com account). I also began firing one cone higher, at cone 03.

Inbound Photo Links


A glaze is crazing. Here is why.
Imagine realizing that pottery you're selling is all going to craze!

Metal leaching from ceramic glazes: Lab report example
Metal leaching from ceramic glazes: Lab report example and a better way

Links

Glossary Liner Glazing
Step-by-step to apply inside and outside glazes to a pottery mug and get them to meet at a clean line at the rim.
Glossary Ceramic Glaze
Ceramic glazes are glasses that have been adjusted to work on and with the clay body they are applied to.
Glossary Base Glaze
Understand your a glaze and learn how to adjust and improve it. Build others from that. We have bases for low, medium and high fire.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Food Safe
Be skeptical of claims of food safety from potters who cannot explain or demonstrate why. Investigate the basis of manufacturer claims and labelling and the actual use to which their products are put.
Tests Thermal Shock Failure
A simple test any potter can do by making and firing square tiles and using a plumbing torch to see how long before they fracture.
Tests 300F:Ice Water Crazing Test
Ceramic glazes that do not fit the body often do not craze until later. This progressively stresses the fit until failure point, thus giving it a score
Media Liner Glazing a Stoneware Mug
I will show you how to glaze a mug with a liner glaze inside and a colored one outside so that they meet in a perfect line at the rim.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy