In ceramics, surface tension is discussed in two contexts: The glaze melt and the glaze suspension. In both, the quality of the glaze surface is impacted.
Key phrases linking here: surface tension - Learn more
In ceramics, the issue of surface tension is most evident in two areas: The glaze melt and slurry rheology.
Surface Tension in Glaze Melts
When a glaze is fired, it melts to form a molten silicate glass. This melt exhibits surface tension, a thermodynamic property that reflects the tendency of the liquid to minimize its surface area. In ceramic glazes, surface tension plays a key role in how the melt wets the clay body, releases gases, and levels during firing and cooling.
Wetting and Spreading: Low surface tension promotes wetting of the clay body and allows the glaze to spread more readily across the surface. High surface tension resists wetting and encourages the melt to contract into thicker regions, contributing to edge pull-back, beading, crawling, and poor coverage.
Bubble Release: Assuming sufficient melt viscosity, surface tension governs how easily gas bubbles rupture at the melt surface. Low surface tension enhances merging and makes bubble films easier to break. High surface tension strengthens the bubble skin, allowing bubbles to persist, reseal, or remain trapped.
Levelling and Surface Smoothness: Surface tension provides the driving force for surface smoothing. However, the extent and rate of levelling are controlled primarily by viscosity (melt mobility). A glaze with high surface tension but low viscosity can still level well, while a glaze with low surface tension but high viscosity may freeze before smoothing is complete. Surface tension helps explain why some glazes pull away from sharp edges while pooling in recesses.
Surface tension in silicate melts is strongly influenced by oxide chemistry, as different oxides alter the structure and ionic bonding of the glass network. A critical caution: many oxides affect surface tension indirectly by changing viscosity and melt structure at the same time, so practical glaze behavior cannot be predicted from surface tension alone.
Oxides commonly associated with higher surface tension (assuming similar melt viscosity, approximate, system- and concentration-dependent). Rightward have higher surface tension and are thus associated with increased melt stiffness, reduced wetting and bubble mobility:
MgO, Al2O3, ZrO2, ZnO, CaO, SnO2, BaO, SrO
Oxides commonly associated with lower surface tension (lowest surface tension rightward; these generally promote wetting, improve levelling, enhance bubble merging and rupture, more gloss):
PbO, B2O3, K2O, Na2O, Li2O
SiO2 forms the glass network and usually raises viscosity strongly, but its effect on surface tension is moderate rather than extreme.
Fe2O3 effects vary strongly with oxidation state, concentration and firing atmosphere.
ZnO is chemically distinctive in that it can function as a strong flux while also increasing melt viscosity, modifying surface behavior and contributing to matte or semi-matte effects in some systems.
ZnO is unusual because it often acts as a flux while simultaneously stiffening melt behavior in certain systems. It can increase crystallization tendency, promote matte surfaces and alter bubble persistence. Its effect is highly composition-dependent.
Practical Implications:
High surface tension + high viscosity: Beading, crawling, poor bubble escape, pinholing, incomplete healing, matte or uneven surfaces.
Low surface tension + low viscosity: Good wetting, smooth levelling, glossy surfaces, good defect healing, possible running.
High surface tension + low viscosity: Can still level well, but may show edge pullback, thick/thin variation, and bubble persistence.
Low surface tension + high viscosity: Implies good coverage, satin surfaces, incomplete levelling if cooling is rapid.
Surface tension is strongly implicated in glaze blistering. Blisters happen where the molten glaze resists bubble rupture at the surface. These or their unhealed remnants often survive to the fired piece when gas pressure inflates the bubble, surface tension maintains the film and viscosity prevents rapid healing after rupture. Strangely, glazes of a more fluid melt can exhibit this problem more, the melt is mobile enough for bubbles to expand, but the surface remains strong enough to hold them. The solution can be a slower cooling through the range at which increasing temperature-induced viscosity has the power to rupture the film. Replacing some higher-surface-tension oxides with lower-surface-tension fluxes often improves blister resistance more effectively than simply increasing melt fluidity.
Surface Tension of Glaze Slurries
On flat surfaces, glaze laydown is not normally an issue, but slurries are suspensions and can resist adhesion and give poor coverage on irregular surfaces (e.g. acute angles, incised or stamped decoration or labelling). Surfactants are available to reduce the surface tension of aqueous glaze systems, they deagglomerate particles and help their homogeneous dispersion over the surface. Polyethylene glycol and Glycerin are considered wetting agents also.

This picture has its own page with more detail, click here to see it.
This cone 04 flow tester compares two commercial low-fire transparent glazes. Their different chemistry strategies are revealed by the shape of these melt flows. While 3825B appears to have the higher melt fluidity, it also has much higher melt surface tension. This is evident in the narrow, rope-like stream and the way the flow meets the runway at a high angle before pulling into a rounded bead. A, by contrast, spreads and wets the runway, meandering downward in a broad, flat and relatively bubble-free river.
This difference is important in low-fire ware because these glazes must pass far more gases and bubbles than high-temperature glazes. The lower surface tension of A aids bubble release and healing after bubbles break. A is Amaco LG-10. B is Crysanthos SG213 (Spectrum 700 behaves similarly, although flowing less). Both approaches have advantages and disadvantages and are worth testing in your application.

This picture has its own page with more detail, click here to see it.
Both are low-fire transparents. In a melt fluidity (GBMF test) they flow similarly. But here, where the 10 gram ball of the dry glaze is simply melted down onto a square tile (a GBMF test), differences in surface tension are more clearly evident by the angle at which the edge of the glaze meets the tile.

This picture has its own page with more detail, click here to see it.
An example of how calcium carbonate can cause blistering as it decomposes during a fast firing in our electric kiln. This is a cone 6 borosilicate glaze with 15% calcium carbonate added (there is no blistering without it). Calcium carbonate has a very high loss on ignition (LOI), and for this early-melting glaze, the gases of its decomposition are still escaping after melting begins. Another factor is also involved: Although the glaze has good melt fluidity, bubbles survived till near the end of the firing, resisting rupture (likely because of the high surface tension of the melt). When the bubbles finally did burst, there was inadequate time for healing to occur.

This picture has its own page with more detail, click here to see it.
These are the same glaze, same thickness, Ulexite-based G2931B glaze, fired to cone 03 on a terra cotta body. The one on the right was fired from 1850F to 1950F at 100F/hr, then soaked 15 minutes and shut off. The problem is surface tension. Like soapy water, when this glaze reaches cone 03 the melt is quite fluid. Since there is decomposition happening within the body, gases being generated vent out through surface pores and blow bubbles. I could soak at cone 03 as long as I wanted and the bubbles would just sit there. The one on the left was fired to 100F below cone 03, soaked half an hour (to clear micro-bubble clouds), then at 108F/hr to cone 03 and soaked 30 minutes, then control-cooled at 108F/hr to 1500F. During this cool, at some point well below cone 03, the increasing viscosity of the melt becomes sufficient to overcome the surface tension and break the bubbles. If that point is not traversed too quickly, the glaze has a chance to smooth out (using whatever remaining fluidity the melt has). Ideally I should identify exactly where that is and soak there for a while.

This picture has its own page with more detail, click here to see it.
An example of how a carbonate can cause blistering. Carbonates produce gases during decomposition. This glaze (G2415B) contains 10% lithium carbonate, which likely pushes the initial melting temperature down toward the most active decomposition temperatures.

This picture has its own page with more detail, click here to see it.
This glaze creates the opaque-with-clear effect shown (at cone 7R) because it has a highly fluid melt that thins it on contours. It is over fired. On purpose. That comes with consequences. Look at the recipe, it has no clay at all! Clay supplies Al2O3 to glaze melts, it stabilizes it against running off the ware (this glaze is sourcing some Al2O3 from the feldspar, but not enough). That is why 99% of studio glazes contain clay (both to suspend the slurry and stabilize the melt). Clay could likely be added to this to increase the Al2O3 enough so the blisters would be less likely (it would be at the cost of some aesthetics, but likely a compromise is possible). There is another solution: A drop-and-soak firing. See the link below to learn more. One more observation: Look how high the LOI is. Couple that with the high boron, which melts it early, and you have a fluid glaze melt resembling an Aero chocolate bar!
![]() High and low melt surface tension: As demonstrated by two pure frits |
![]() Gummed dipping glazes can dry like this: How to fix it. |
| Articles |
A Low Cost Tester of Glaze Melt Fluidity
Use this novel device to compare the melt fluidity of glazes and materials. Simple physical observations of the results provide a better understanding of the fired properties of your glaze (and problems you did not see before). |
| Recipes |
G3806C - Cone 6 Clear Fluid-Melt transparent glaze
A base fluid-melt glaze recipe developed by Tony Hansen. With colorant additions it forms reactive melts that variegate and run. It is more resistant to crazing than others. |
| Glossary |
Rutile Blue Glazes
A type of ceramic glaze in which the surface variegates and crystallizes on cooling in the presence of titanium and iron (usually sourced by rutile) |
| Glossary |
Fluid Melt Glazes
Fluid melt glazes and over-melting, over fired, to the point that they run down off ware. This feature enables the development of super-floss and cyrstallization. |
| Glossary |
Ceramic Glaze Defects
Ceramic glaze defects include things like pinholes, blisters, crazing, shivering, leaching, crawling, cutlery marking, clouding and color problems. |
| Glossary |
Melt Fluidity
Ceramic glazes melt and flow according to their chemistry, particle size and mineralogy. Observing and measuring the nature and amount of flow is important in understanding them. |
| Glossary |
Glaze Bubbles
Suspended micro-bubbles in ceramic glazes affect their transparency and depth. Sometimes they add to to aesthetics. Often not. What causes them and what to do to remove them. |
| Glossary |
Glaze Crawling
A ceramic glaze fault that occurs during firing of the ware, the molten glaze pulls itself into islands leaving bare patches of body between. |
| Glossary |
Glaze Blisters
Blistering is a common surface defect that occurs with ceramic glazes. The problem emerges from the kiln and can occur erratically in production. And be difficult to solve. |
| URLs |
https://en.wikipedia.org/wiki/Surfactant
Surfactants at Wikipedia |
| URLs |
https://www.zschimmer-schwarz.com/en/ceramic-auxiliaries/tiles/glaze-additives/wetting-agents
Wetting agents from zschimmer-schwarz.com: Surfactants that reduce the surface tension of aqueous glaze systems. |
| Troubles |
Crawling
Ask yourself the right questions to figure out the real cause of a glaze crawling issue. Deal with the problem, not the symptoms. |
| Troubles |
Glaze Blisters
Questions and suggestions to help you reason out the real cause of ceramic glaze blistering and bubbling problems and work out a solution |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk