Ag2O | AlF3 | As2O3 | As4O6 | Au2O3 | BaF2 | BeO | Bi2O3 | CaF2 | CdO | CeO2 | Cl | CO | CrO3 | Cs2O | CuCO3 | Dy2O3 | Er2O3 | Eu2O3 | F | Fr2O | Free SiO2 | Ga2O3 | GdO3 | GeO2 | HfO2 | HgO | Ho2O3 | In2O3 | IrO2 | KF | KNaO | La2O3 | Lu2O3 | Mn2O3 | MoO3 | N2O5 | NaF | Nb2O5 | Nd2O3 | Ni2O3 | OsO2 | Pa2O5 | PbF2 | PdO | PmO3 | PO4 | Pr2O3 | PrO2 | PtO2 | RaO | Rb2O | Re2O7 | RhO3 | RuO2 | Sb2O3 | Sb2O5 | Sc2O3 | Se | SeO2 | Sm2O3 | Ta2O5 | Tb2O3 | Tc2O7 | ThO2 | Tl2O | Tm2O3 | Trace | U3O8 | UO2 | WO3 | Y2O3 | Yb2O3

BaO (Barium Oxide, Baria)

Data

Co-efficient of Linear Expansion 0.129
Frit Softening Point 1923C

Notes

-Together with CaO, SrO, and MgO it is considered one of the alkaline earth GROUP of oxides. It has a cubic crystal structure and is the heaviest of the divalent fluxing oxides.

-BaO is most commonly employed in pottery as a matting agent with good color response (e.g. with copper it will give a marked blue compared to glazes fluxed with MgO, SrO).

-BaO often contributes a high index of refraction and this can enhance and brighten in-glaze colors. It is recommended for celadons but not iron reds or chrome greens.

-As a flux it can be very active in small amounts (not active at low temperatures). For example, it can improve gloss, elasticity, mechanical strength, corrosion resistance, and acid resistance.

-Barium imparts properties to glazes that fall between calcia/magnesia and lead (it tends to produce a denser, more brilliant but less durable product than calcia). Barium does not reduce in the melt and therefore does not discolor. It acts as a flux (if decomposed) and can assist in the formation of a matte structure. Barium forms silicates slowly, but when completely combined it is very active as a fluxing agent.

-Baria is more effective as a melter when associated with other fluxing oxides with which it can combine (e.g. if fused in certain frit formulations it can react readily in even low temperature glazes). It is known, for example, to form a strong eutectic with B2O3 to produce glossy and runny glazes that can solidify below 500C).

-In larger amounts it becomes refractory and can produce leachable glazes (since it does not fully combine to form insoluble silicates). It is common to see art glazes with more than 20% barium carbonate, and at times, even 40-50% recipes are traded in the pottery community. These are almost certainly leachable.

-Use with caution in functional ware! There is considerable controversy concerning the safety of barium in glazes (i.e. if you see larger amounts of barium in glazes labeled 'Dry Matte' or 'Stony Matt', be very cautious). Like lead, it can be leached FROM the surface (of improperly fired or formulated glazes) by acidic foods or liquids.

-If possible, determine the reason for BaO in the recipe. The mechanism may well be better accomplished by another oxide. For example, SrO and CaO can both be employed to produce crystal mattes in saturation (both are smoother to the touch). K2O may produce a better blue with copper or a brighter color.

-SrO has been promoted as a glaze substitute for BaO and in some cases this is true. It has a lower disassociation temperature and reacts earlier and is potentially able to produce a more perfect surface (unmarred by the bubbles and pits associated with higher temperature decomposition). Still it is best to substitute BaO on a 'mechanism' basis, that is, understand why it is there and choose the best alternate oxide based on that. In some cases.

-Used in optical glass (up to 30%),
-Used in small amounts in bottle and flat glass (.5%),
-It was in common use in glass formulations in the television tube industry.
-It can produce better translucency in porcelain bodies.
-It is used to provide maximum flux density in hard-core permanent magnets.
-In enamels its acts as a strong flux and is less expensive than lead or zinc. It does not reduce in the presence of iron high in carbon however it is sensitive to the presence of sulfur (i.e. an impurity in antimony).
-Used in pressed glass tableware it renders brilliance and finish, but detrimentally affects certain other mechanical properties.

Ceramic Oxide Periodic Table

Periodic table of ceramic oxides

Pretty well all common traditional ceramic base glazes are made from less than a dozen elements (plus oxygen). Go to the full picture of this table and click or tap each of the oxides to learn more (on its page at digitalfire.com). When materials melt, they decompose, sourcing these elements in oxide form. The kiln builds the glaze from them, it does not care what material sources what oxide (assuming, of course, that all materials do melt or dissolve completely into the melt to release those oxides). Each of these oxides contributes specific properties to the glass. So, you can look at a formula and make a good prediction of the properties of the fired glaze. And know what specific oxide to increase or decrease to move a property in a given direction (e.g. melting behavior, hardness, durability, thermal expansion, color, gloss, crystallization). And know about how they interact (affecting each other). This is powerful. A lot of ceramic materials are available, hundreds - that is complicated when individual materials source multiple oxides. Viewing a glaze as a simple unity formula of ceramic oxides is just simpler.

Substituting MgO for BaO in a matte will also make a matte, right? Wrong.


This picture has its own page with more detail, click here to see it.

Left: G2934 magnesia cone 6 matte (sold by Plainsman Clays). Right (G2934D): The same glaze, but with 0.4 molar of BaO (from Ferro Frit CC-257) substituted for the 0.4 MgO it had. The MgO is the mechanism of the matte effect. Barium also creates mattes, but only if the chemistry of the host glaze and the temperature are right. In addition, barium mattes are normally made using the raw carbonate form, not a frit. In fritted form, barium can be a powerful flux when well dissolved in the melt and boron is present. This glaze is actually remarkably transparent. However, if this was fired lower it could very well matte.

Links

Glossary Limit Formula
A way of establishing guideline for each oxide in the chemistry for different ceramic glaze types. Understanding the roles of each oxide and the limits of this approach are a key to effectively using these guidelines.
Glossary Alkaline Earths
Refers to a group of ceramic fluxing oxides that contribute similar properties to fired glazes. They contrast with the alkalis which are stronger fluxes.
Glossary Flux
Fluxes are the reason we can fire clay bodies and glazes in common kilns, they make glazes melt and bodies vitrify at lower temperatures.
Oxides SrO - Strontium Oxide, Strontia
Materials Barium Frits
Materials Barium Nitrate
Materials Barium Sulfate
Materials Barium Carbonate
A pure source of BaO for ceramic glazes. This is 77% BaO and has an LOI of 23% (lost at CO2 on firing).
Hazards Barium Carbonate in Clay Bodies
Considerations regarding the use of barium carbonate in pottery and structural clay bodies for precipitation of soluble salts.

Mechanisms

Glaze ColorBarium glazes are well known for thier ability to produce matte turquoise colors with copper. While strontium is often used to duplicate the matte texture of barium it does not have the same color response.
Glaze MattenessBaria is well known for its tendency to cause the growth of a fine mesh of micro crystals to produce a silky matte texture.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy