0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Translucency

A highly sought-after property in porcelain, fired close enough to melting to take on the glass-like property of passing light. Translucency implies tendency to warp during firing.

Key phrases linking here: translucency, translucent - Learn more

Details

Photo not found
or not published

Translucent porcelain enables the passage of light through the wall of the item. Anorthite porcelain (bone china) is more translucent than traditional mullite porcelain. Highly vitreous porcelains are needed. Unfortunately, they don't maintain their shape during firing. To resolve this problem with bone china, bisque firing is done in holders and setters, and pieces are finished using glazes that melt at lower temperatures. In recent years, the availability of white-burning plasticizers has made it possible to maximize feldspar content in even potter's porcelains, resulting in translucency in mullite ware that seems to go beyond the theoretical.

Thus today, most companies find the traditional bone-china process to be unnecessary in producing a super-white translucent porcelain. But there are more factors at play to produce translucency in non-bone-china porcelain than it might at first appear. Of course, it is well known that kaolins containing significant titanium impede translucency. Thus, the most sought-after kaolins are those with low TiO2 and low iron content (Grolleg and New Zealand china clay are examples). It seems obvious that bodies need to be fired to a point well past where they reach zero porosity to have really good translucency. But this is not necessarily true. It also seems obvious that the range within which good translucency happens, and ware is stable enough to hold itself in shape during firing, would be very narrow. Again, this is not necessarily true. Using frits as a flux also seems obvious to achieving really good translucency, but this is not necessarily true either, feldspar-only porcelains can be very translucent. Also, as noted and contrary to what many people believe, high temperatures (cone 10 and beyond) are not required for good translucency.

The recipe for a cone 10 translucent plastic porcelain is really quite simple: It needs 20-25% silica for glaze fit. It needs 2-4% white bentonite (e.g. VeeGum, Bentone) for workability. 25% feldspar (high-quality low iron) will give less fired warping and less translucency, 35% will give the best translucency and the least stability in the kiln. The rest of the recipe is high-quality white-burning kaolin (e.g. New Zealand). For a casting version, cut the bentonite to 1% or less (just enough to impart the plastic strength needed to pull away from the mold). Some white kaolins (e.g. English) contain significant fluxes so less feldspar is needed (up to 10% less), this enables higher kaolin and/or silica percentages.

Cone 6 porcelains are more of a challenge because more feldspar is needed (leaving less room for kaolin in the recipe). Here is one secret of how to achieve translucency at cone 6: Veeum T. The L3778D recipe is an example of its use. Although not advertised by its manufacturer and not known by them, Veegum imparts translucency when used in larger amounts (up to 4%), so much less feldspar is needed (we have achieved excellent translucency with as little as 20%). Of course, it is very expensive; that 4% will cost more than the other 96% of the ingredients. The low-iron, low-titanium kaolins are not plastic, so they produce porcelain bodies of poor working properties. But the Veegum more than makes up for that, producing body workability that seems impossible for the whiteness and translucency achieved. We have not found frits to work nearly as well as Veegum.

Photo not found
or not published

For low temperatures, frits are the only answer to achieving translucency. Fritware bodies take the "crowbar approach" by simply increasing the percentage of glass in the matrix. They can mature as low as cone 06 (or even lower) if you can afford the frit. We have found Ferro Frit 3110 works well, our Zero3 porcelain is an example. It might seem that pieces made in such a way would simply warp or collapse during firing, but that is not the case. Even very thin slip cast pieces can be fired with little warping (provided they have a stable shape), we have fired cold-to-cold in a standard pottery kiln, in three hours. Potters now have controller-equipped kilns and can develop a firing schedules that strike a balance of maturity/translucency and resistance to warping for any recipe. Or, they can tune the recipe to develop to the desired degree at a target temperature.

Of course, glazes and engobes can also be translucent, depending on the degree of melt and the presence of opacifiers, colorants and crystallization.

Related Information

The translucency of Polar Ice porcelain


A slab-built porcelain mug with yellow glaze showing off its translucency in sunlight

This picture has its own page with more detail, click here to see it.

Polar Ice is made by Plainsman Clays, it is by far the most expensive body they make (because of the use of New Zealand kaolin and VeeGum). I call these my "sunshine mugs". They are fired at cone 6 (2200F) with a transparent glaze on the inside (G2926B) and G2934Y yellow silky matte on the outside (both mixed and applied at dipping glazes). This yellow glaze showcases the translucency in sunlight better than any other I have seen. The high plasticity and this "pie crust" method of making them enable thinner walls than any other method I know of, even casting. Although the walls of this piece are about 3.5 mm thick, I have achieved 2 mm using stiffer clay! Even with very thin walls, the weight of the handle does not pull the lips of these into an oval-shape.

Grolleg vs New Zealand - Which kaolin is better for translucency?


Two translucent mugs

This picture has its own page with more detail, click here to see it.

The NZK body, Polar Ice, is on the left. The Grolleg one, L3778D, is on the right. They are not the same recipe, the feldspar content in the L3778D has been adjusted to match the degree of vitrification (Grolleg contains some feldspar). Clearly, the NZK has better translucency. And it fires whiter.

The sun. Brought to you by Plainsman Polar Ice!


This picture has its own page with more detail, click here to see it.

The walls are very thin, yet no trimming was done to make them thin. Why? It is super plastic. Others claim to be plastic, but they use the word in a relative sense. They mean a little less flabby than other flabby porcelains! Polar ice, when it has the right water content (dewater it on a bat if needed), is tough enough to throw as large as even the most plastic stonewares. It might seem impossible that a body this translucent can be as plastic as it is and as stable in the kiln as it is. Want to know it’s recipe? Search around on this site and you will find clues in a number of places, put them together, do a little testing, and derive it yourself!

Translucent Porcelain Lithophane by Stephanie Osser


This picture has its own page with more detail, click here to see it.

Made using porcelain fired to cone 11+. This is a splendid demonstration of translucency. Without a back-light it is just a white slab. But the varying thickness in the porcelain determine the amount of light that passes at any given spot, thus producing the design. An example of a recipe to produce a porcelain like this is L3778D.

A Lithophane exploits porcelain translucency to reveal its design


This picture has its own page with more detail, click here to see it.

Top: A thin porcelain tile with etched design. Bottom: The same tile with a back light. By Stephanie Osser. L3778G is an example of a translucent mullite porcelain that will work for this.

Reduction Polar Ice vs. Oxidation Polar Ice


This picture has its own page with more detail, click here to see it.

Polar Ice (Plainsman Clays) has been fired to cone 10R (left). This is beyond the recommended cone 6 range, but it worked well in this instance. The result is even more translucency and a translucency of a different character: blue! This looks much more like real blue polar ice.

Translucency of Polar Ice compared to another porcelain at cone 6


This picture has its own page with more detail, click here to see it.

On the top you can see the color difference. The other porcelain is made from a low TiO2 mix of typical North American kaolins, feldspars and bentonites. Bottom with a light inside: Polar ice on the left is far more translucent. Yet it is not overly mature, it resists fired warping remarkably well. And it is also more plastic (which seems impossible). There is a secret to the translucency that goes beyond the fact that it employs New Zealand kaolin and the percentage of feldspar it has. But I cannot tell you. But if you read this site carefully you will discover it in the most unlikely place!

Polar Ice casting translucency


This picture has its own page with more detail, click here to see it.

A bowl cast from Polar Ice porcelain and fired to cone 6. I has a thinner wall than the thrown pieces made from Polar Ice throwing, yet it is much less translucent. This appears to be because the VeeGum is much less.

The secret of this cone 6 translucency will surprise you!


This picture has its own page with more detail, click here to see it.

Three cone 6 mugs. All have zero porosity. Why is the middle one so translucent? Three reasons.
1. It has 10% more feldspar than the one on the left and reaches zero porosity already at cone 5.
2. It employs New Zealand china clay while the one on the left contains high-TiO2 #6 Tile kaolin.
But this is also true for the one on the right. The third difference is the key.
3. The center one contains 4% Veegum T plasticizer (while the other two use standard bentonite). This is surprising when I tell you one more thing: The mug on the right also contains 3% Ferro Frit 3110. That means that the frit does not have near the fluxing power of the VeeGum!

Want to make a cone 10R super translucent porcelain? Think again.


This picture has its own page with more detail, click here to see it.

On the right is a porcelain used in China, renowned for its whiteness and translucency. On the left is a body made from Grolleg kaolin, this is commonly used by potters. They were fired in reduction. The tiny iron specks that potters do not even notice are enemy number for the blue-white porcelain like this. Although they might be small the reduction atmosphere makes them blossom out in full glory to ruin the piece. These specks come as contaminants in the materials (especially the silica) and they are easily picked up during fabrication. For very white bodies like this, it is incredibly difficult to prevent the specks. For a perfectly white flawless result, the entire factory must be dedicated to this one body; they use wet processing, magnets, filter pressing, stainless steel equipment and impeccable procedures.

Inbound Photo Links


Produced by Gemini, combining a picture of a mug I made with a generated bone china one. AI Policy
Mullite and anorthite porcelains: The microstructure was only understood recently

Links

Glossary Porcelain
How do you make porcelain? There is a surprisingly simple logic to formulating them and to adjusting their working, drying, glazing and firing properties for different purposes.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Bone China
A ceramic whose priorities are translucency, whiteness, fired strength and resistance to thermal shock failure.
Glossary Vitrification
A process that happens in a kiln, the heat and atmosphere mature and develop the clay body until it reaches a density sufficient to impart the level of strength and durability required for the intended purpose. Most often this state is reached near zero p
URLs https://insight-live.com/insight/share.php?z=tgsPMxNsAP
Four Cone 6 (1200C) Casting/Throwing Porcelain Recipes (Grolleg and #6 Tile)
Four recipes that can be adjusted to work for casting or throwing/hand building (by adjusting the percentage of bentonite). The more you are willing to spend on the materials the more whiteness, translucency and plasticity you will achieve.
URLs https://www.amacusabotao.com/
Individually handcrafted garment buttons made from translucent porcelain.
URLs https://en.wikipedia.org/wiki/Herend_Porcelain_Manufactory
Herend Translucent Porcelain

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy