0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Flux

Fluxes are the reason we can fire clay bodies and glazes in common kilns, they make glazes melt and bodies vitrify at lower temperatures.

Key phrases linking here: fluxed, flux - Learn more

Details

Fluxes are materials that lower the melting temperature of a glaze or the vitrification range of a clay body. More correctly, materials contain certain oxides that act to lower the melting or softening temperature of a mix of materials. Fluxes are interactors (they often melt poorly on their own but react strongly with high-melting materials where Al2O3/SiO2 predominate). There are less than ten common fluxes that we need to be concerned with. When we discuss them, we are talking about specific oxides (not powdered materials). Fluxes are sourced by the materials in the recipe, they are "swimming around" in the glaze melt during firing, making it fluid, giving it the ability to dissolve other particles within and without.

During firing, fluxes interact with the surface molecular structure of raw and refined materials and pull them away (dissolve them) molecule-by-molecule. Glaze chemistry considers how each of the oxides, as individuals, impose their properties on the glass (is assumes they have all melted or dissolved). But it also tries to understand how they interact with each other (e.g. sometimes combinations of fluxes react much more than logic would expect). Normally, the more kinds of fluxes present in a mix the lower its melting temperature (called the 'mixed oxide effect'). Interactions between fluxing oxides trigger on percentages, identities and mixtures of identities, temperature and kiln atmosphere (it is a lifetime of study).

Glazes made from raw materials that source fluxing oxides (like feldspar, calcium carbonate, talc, dolomite) have flux balances that mirror what is common in rocks on the planet. These melt well at high stoneware temperatures. If we add Gerstley borate or Colemanite (which introduce B2O3) and metal oxides and carbonates (like zinc, lithium, strontium) it is possible to move melting temperatures way down and create a broader range of effects. Finally, by adding frits (artificial materials which release their fluxes more readily and that offer proportions that cannot be achieved with common materials) we can lower temperature even further and create very novel effects. Generally it is best to use as many fluxes in a glaze as possible, both to benefit from the mixed-oxide-effect, and have more options to adjust and tune the recipe.

In common glazes, the fluxing oxides comprise a minor percentage (compared to SiO2 and Al2O3). A high-temperature (1300C) stoneware glaze might have 18% fluxes. A middle-fire (1180C) stoneware might contain 22%. A low fire glaze might have 30% flux (including B2O3). This is a narrower range of percentages than one would expect, but we can explain it by the varying potency of the fluxing oxides and the fact that certain oxides predominate in each temperature range. Of course, certain fluxes are supplied by materials that are much more expensive than others.

B2O3 is a special-case flux. It acts as a low-melting glass (it does not depend on percentage and interaction to activate). It works across the entire temperature range used in traditional ceramics. Much of the ceramic industry would not exist without this valuable oxide. Almost all frits contain at least some B2O3. It is common to see 15% B2O3 in low fire glazes. At middle temperature, 5% B2O3 is common (reactive glazes could have more). But if ZnO and significant KNaO are present, B2O3 could be around 2%. In high fire glazes there is almost always zero boron.

PbO is also a special case since, although it is a highly effective melter at low temperatures, it is no longer used in most circles because of toxicity concerns.

Li2O and ZnO are strong fluxing oxides, they work well at lower temperatures (but must be used judiciously at higher ones to avoid overmelting and volatilization). Glazes employ fairly small amounts of these in combination with other fluxes (except for some zero-boron glazes that employ zinc as the power-melter). Over-supplying either of these, especially at higher temperatures, can result in radical changes in color and surface characteristics. In stoneware and porcelain glazes it is common to see zero ZnO and LiO2.

At higher temperatures a new set of fluxes burst onto the scene: K2O and Na2O (commonly deemed KNaO), CaO, BaO, SrO, MgO. Although you will find these oxides in glazes at all temperatures, they are much less active at the lower. An exception is KNaO, very active at all ranges but restricted in the amount allowable because of its high thermal expansion (KNaO is very effective at fostering high gloss and brilliant colors). CaO is the most common fluxing oxide found at all temperature ranges (commonly 5-10% of the total). Actually, that is not entirely true. Although it reacts strongly (is very effective) at high temperatures, it is simply present in lower-fire glazes, acting more as an intermediate (in fact, it can be a matting agent at low fire). CaO is just there. It is in the raw materials and frits we use (it is in the rocks on this planet). It is not a troublesome oxide (unless in very high amounts where it mattes by crystallizing). MgO is also common in glazes (since dolomite and talc, its sources, are so commonly used). MgO has very low thermal expansion, trading it against higher expansion fluxes is an effective way to deal with crazing. Using it as a predominant flux at middle and high temperatures produces a silky matte surface (while still melting well). SrO and BaO are used in smaller amounts (the latter normally for special colors or to produce micro-crystalline matte surfaces).

Colorants can also be powerful fluxes. Copper, cobalt and manganese all melt very actively in oxidation and reduction. However iron, a refractory material in oxidation, is a strong flux in reduction.

When the term flux is used on the material level, it is referring to the fact that the chemistry of the material contributes a significant amount of one or more of the fluxing oxides. Feldspar is an excellent example of a natural mix of refractory SiO2 and Al2O3 and fluxing oxides that, together, melt at a fairly low temperature. However, raw materials commonly as glaze fluxes, do not always melt well by themselves. Dolomite, like calcium carbonate, is a stoneware glaze fluxing material. But by itself it can be dead-burned and used as a heavy-duty refractory for ladles and slag furnaces! Talc, in small percentages in middle temperature clay bodies, acts as a strong flux. However, in large percentages, it is refractory also. Calcium carbonate is another example. While being a strong glaze flux at higher temperatures, it is refractory in a 75:25 plastic mix with bentonite (where the conditions for interaction to produce a glass are not present).

Fluxing oxides in frits melt much better than in raw materials. MgO is an excellent example. Glazes that employ a frit to supply the MgO melt much better than those employing dolomite or talc. SrO is a similar story.

Understandably, predicting the effects of a flux addition to a glaze (e.g. melting temperature) is very complex (involving interactions, eutectics, proportions, premelting, atmostphere and the physical and mineralogical properties of the particles). For this reason, glaze chemistry is applied much more in a relative sense than absolute to predict melting temperature.

Related Information

Pure stain powders painted overglaze:

Why the bleeding and bubbling?


Stains used pure as overglazes don't work

This picture has its own page with more detail, click here to see it.

The blue is melting and bleeding profusely into the glaze. The green is the opposite - refractory, stiffening the glaze enough to trap bubbles and sit on the surface as a dry, unmelted layer. Under the glaze, these problems would be magnified (the blue bleeding more, the green causing crawling and blistering).

Stains are not ceramic; they are ceramic additives. Stains are not considered safe for direct food contact. Stains are expensive. Stains don't suspend in water, paint poorly and dry as a loose powder.

Both of these (and others) need to be added, as a minor percentage, to a ceramic carrier (one with CMC gum and a mix of ceramic materials tailored to melt to the desired degree and have a compatible chemistry to develop the color (as per manufacturer guidelines).

A highly fluxed body, when over fired can do this!


This picture has its own page with more detail, click here to see it.

These two mugs are made from the same material: Ravenscrag Slip plus 20% Ferro Frit 3134. The one on the right has been bisque fired to 1550F. The one on the left has been clear glazed and fired to cone 03 (1950F). That means that this body vitrifies well below cone 03, likely well below cone 06. Thus strength, maturity, vitrification are not a matter of temperature, they are a matter of how much flux is available in the body to mature it to a dense, strong matrix.

Copper is not just a pigment:

It can be a powerful flux, with consequences


This picture has its own page with more detail, click here to see it.

Left: The base recipe of GA6-C (80% Alberta Slip, 20% Frit 3134, 4% rutile). That recipe is stable; it does not run. Right: A 2% addition of copper carbonate transforms it into a runny, melt fluid glaze. It also produces a pleasant green even on this red-burning body (a good green is not easy in oxidation ceramics). Using a catch glaze (e.g. a frit-reduced version), this could be made safe on vertical surfaces. However, there are red flags here. Having only 2% copper would not destabilize a typical glaze (making it leachable). But phase separation is occurring here, likely because the base contains significant rutile. That means the phases are copper-bearing and possibly copper-concentrating. And, as noted, the copper has a greater-than-expected impact on the melt. Third, commercial variegated copper glazes can even leach in acids (as happened with the mug inset after a night with lemon juice). While the GA6-C recipe does have a 0.3:0.7 R2O:RO ratio, other indicators make it a course of wisdom to consider the GLLE test before use on functional surfaces.

Copper fluxes a matte glaze at cone 6


This picture has its own page with more detail, click here to see it.

4% copper carbonate and 6% rutile have been added to G2934 cone 6 matte base. Using a green stain should prevent this. Or some B2O3 could be substituted with SiO2 (via glaze chemistry).

Iron oxide goes crazy in reduction


This picture has its own page with more detail, click here to see it.

Cone 6 iron bodies that fire non-vitreous and burn tan or brown in oxidation can easily go dark or vitreous chocolate brown (or even melting and bloated in reduction). On the right is Plainsman M350, a body that fires light tan in oxidation, notice how it burns deep brown in reduction at the same temperature. This occurs because the iron converts to a flux and the glass development that occurs brings out the dark color. On the left is Plainsman M2, a raw high iron clay that is quite vitreous in oxidation, but in reduction it is bloating badly. When reduction bodies are this vitreous there is a much great danger of black coring.

The amazing fluxing power of boron (in borax)


This picture has its own page with more detail, click here to see it.

The two top clay bars contain 15% hydrous borax. At cone 06, a very low temperature, it has already melted and drained out of the bars, running down over the others as a glass.

Trying to avoid knowing anything about glaze chemistry? Be ready for drama!


A periodic table of oxide with elements important to ceramics highlighted

This picture has its own page with more detail, click here to see it.

Maybe you don't think it is necessary to know anything about glaze chemistry to be a potter. Or a technician at a production facility. This thinking depends on how much mystery you mind tolerating. Because the reason for many of the problems you will encounter with glazes relates fundamentally to their chemistry. Perhaps you have other "social" actors in your sphere who also specialize in the "know as little technical stuff as possible" mindset. Who treat glazes like acrylic paint that comes in tubes - it is just color! From these people, you will get buying advice on expensive jars of tacky-looking "goop" that you have to laboriously paint on in layers. Or it will mean you'll be more likely to get trapped on the recipe treadmill, addicted to the traffic of recipes that never seem to work.

Add 5% calcium carbonate to a tenmoku. What happens?


This picture has its own page with more detail, click here to see it.

In the glaze on the left (90% Ravenscrag Slip and 10% iron oxide) the iron is saturating the melt crystallizing out during cooling. GR10-K1, on the right, is the same glaze but with 5% added calcium carbonate. This addition is enough to keep most of the iron in solution through cooling, so it contributes to the super-gloss deep tenmoku effect instead of precipitating out.

Firing shrinkage variation between various clays


This picture has its own page with more detail, click here to see it.

Example of various materials mixed 75:25 with volclay 325 bentonite and fired to cone 9. Plasticities and drying shrinkages vary widely. Materials normally acting as fluxes (like dolomite, talc, calcium carbonate) are refractory here because they are fired in the absence of materials they react normally with.

Frits work much better in glaze chemistry


This picture has its own page with more detail, click here to see it.

The same glaze with MgO sourced from a frit (left) and from talc (right). The glaze is 1215U. Notice how much more the fritted one melts, even though they have the same chemistry. Frits are predictable when using glaze chemistry, it is more absolute and less relative. Mineral sources of oxides impose their own melting patterns and when one is substituted for another to supply an oxide in a glaze a different system with its own relative chemistry is entered. But when changing form one frit to another to supply an oxide or set of oxides, the melting properties stay within the same system and are predictable.

How do metal oxides compare in their degrees of melting?


Metal oxides melting

This picture has its own page with more detail, click here to see it.

These metal oxides have been mixed with 50% Ferro frit 3134 and fired to cone 6 oxidation. Chrome and rutile have not melted, copper and cobalt are extremely active melters, frothing and boiling. Cobalt and copper have crystallized during cooling. Manganese has formed an iridescent glass.

Frits melt so much better than raw materials


Frits, talc, feldspar melting

This picture has its own page with more detail, click here to see it.

Feldspar and talc are both flux sources (glaze melters), they are common in all types of stoneware glazes. But their fluxing oxides, Na2O and MgO, are locked in crystal structures that neither melt early or supply other oxides with which they like to interact. The pure feldspar is only beginning to soften at cone 6. Yet the soda frit is already very active at cone 06! As high as cone 6, talc (the best source of MgO) shows no signs of melting activity at all. But a high-MgO frit is melting beautifully at cone 06! The frits progressively soften, starting from low temperatures, both because they have been premelted and have significant boron content. In both, the Na2O and MgO are free to impose themselves as fluxes, actively participating in the softening process.

At 1550F Gerstley Borate suddenly shrinks!


This picture has its own page with more detail, click here to see it.

These GBMF test balls were fired at 1550F and were the same size to start. The Gerstley Borate has suddenly shrunk dramatically in the last 40 degrees (and will shrink even more and then suddenly melt down flat within the next 50). The talc is still refractory, the Ferro Frit 3124 slowly softens across a wide temperature range. The frit and Gerstley Borate are always fluxes, the talc is a flux under certain circumstances.

2% Copper in two cone 6 transparents:

One does not bubble and orange-peel. Why?


This picture has its own page with more detail, click here to see it.

The top base glaze, G2926B, has enough melt fluidity to produce a brilliant functional gloss when used as a transparent. However, for this 2% copper carbonate addition, it has too little melt fluidity and/or too much surface tension to merge, pass and heal the entrained micro-bubbles (generated by the decomposition of the carbonate).

The lower glaze, G3806B, diversifies the fluxes (half the B2O3 in exchange for more Na2O and introduction of SrO and ZnO) and increases their total compared to Al2O3 and SiO2. The result is a more fluid cone 6 melt having lower surface tension. The mixed-oxide effect is also a factor here; the diversity itself improves the melt.

The above factors are enough to solve the problem here. But more can be done. More zinc (in exchange for KNaO) could produce later melting, especially in combination with sourcing some or all of the latter from a feldspar instead of the low-melting frit. The benefit would enable more gas escape until melt-sealing (and reduce the COE).

Inbound Photo Links



Stains having varying fluxing effects on a host glaze

Links

Typecodes Flux Source
Materials that source Na2O, K2O, Li2O, CaO, MgO and other fluxes but are not feldspars or frits. Remember that materials can be flux sources but also perform many other roles. For example, talc is a flux in high temperature glazes, but a matting agent in low temperatures ones. It can also be a flux, a filler and an expansion increaser in bodies.
Oxides MgO - Magnesium Oxide, Magnesia
Oxides SrO - Strontium Oxide, Strontia
Oxides BaO - Barium Oxide, Baria
Oxides B2O3 - Boric Oxide
Oxides ZnO - Zinc Oxide
Oxides Na2O - Sodium Oxide, Soda
Oxides Li2O - Lithium Oxide, Lithia
Oxides K2O - Potassium Oxide
Oxides CaO - Calcium Oxide, Calcia
Troubles Runny Ceramic Glazes
Glazes of high melt fluidity are likely to run if applied to thickly or have not catcher glaze
Glossary Refractory
In the ceramic industry, refractory materials are those that can withstand a high temperature without deforming or melting. Or can be sintered into super materials.
Glossary Frit
Frits are used in ceramic glazes for a wide range of reasons. They are man-made glass powders of controlled chemistry with many advantages over raw materials.
Glossary Limit Formula
A way of establishing guideline for each oxide in the chemistry for different ceramic glaze types. Understanding the roles of each oxide and the limits of this approach are a key to effectively using these guidelines.
Articles What Determines a Glaze's Firing Temperature?
The oxides contributed by glaze materials determine its chemistry. The chemistry is the main factor determining melting behaviour. But the particle sizes, shapes and mineralogies also come in to play.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy