Magnesia matte ceramic glazes are “microstructure mattes” while calcia mattes are “crystal mattes”. They have a micro-wrinkle surface that forms from a high viscosity melt and microscopic phase separation, both of which prevent levelling on freezi
Key phrases linking here: magnesia mattes, magnesia matte, mgo matte - Learn more
Photo not found
or not published

This picture has its own page with more detail, click here to see it.
This melt flow test was done at cone 6+ (without slow cooling) to demonstrate the difference in melt viscosity between a calcia matte (left G1214Z1) and a magnesia matte (right G2928C). In simplest terms, the former depends on a fluid melt to provide the needed mobility for tiny crystals to form during cooling, those crystals scatter the light and soften the surface to produce the matte effect. The latter requires a stiffer melt to help prevent levelling during cooling and host phase separation to produce a rippled surface that scatters light.

This picture has its own page with more detail, click here to see it.
I am looking to match the reduction-fired dolomite matte mug on the right, but in cone 6 oxidation. I must duplicate the glaze color and surface character. But more difficult is the speckle size, color, density and edge bleeding. The speckle is the biggest challenge, but I met that by making my own by mixing the body and G2926B glossy glaze 50:50 and adding 10% black stain. Then I slurry it, dry it, fire it in a crucible (which I make from L4404A with an L3693E liner), crush it by hand using my shusher and screen it. I am using G2934 cone 6 magnesia matte as the glaze on this mug on the left. I add 0.5% minus 20 mesh speck to achieve this result. The next step in this project is to sieve out the smallest specks, switch to the G2934 matte glaze in the speckle recipe (the specks are too shiny here), and switch to dark brown stain instead of black. I will also need to control the degree to which the specks bleed at their edges (by adjusting the glaze:body ratio) and tune the degree of matteness (by adjusting cooling speed of the kiln). A small amount of green or blue stain is also needed to match the glaze color. There is no question that an authentic reproduction is possible; methodical testing with good records is the key to accomplishing that.

This picture has its own page with more detail, click here to see it.
Matte glazes have a fragile mechanism. That means the same recipe will be more matte for some people, more glossy for others (due to material, process and firing differences). In addition, certain colors will matte the base more and others will gloss it more. It is therefore critical for matte glaze recipes to have adjustability (a way to change the degree of gloss), both for circumstances and colors. This recipe is Plainsman G2934 base matte with 6% Mason 6600 black stain added. It has been formulated to be on the more matte side of the scale so that for most people a simple addition of G2926B (M370 transparent ultra clear base recipe) will increase the gloss. That means users need to be prepared to adjust each color of the matte to fine-tune its degree of gloss. Here you can see 5:95, 10:90, 15:85 and 20:80 blends of the matte:gloss recipe bases.

This picture has its own page with more detail, click here to see it.
These are 10 gram GBMF test balls that we melted on porcelain tiles at cone 4 (top two) and cone 6 (bottom two). They compare the melt fluidity of G2934 (left) and G2934Y (right). The Y version sources its MgO from frit and talc (rather than dolomite). It is a much more fluid melt because the frit is yielding the oxides more readily. But Y has a key benefit: It has a much lower LOI, producing fewer entrained air bubbles and therefore fewer surface defects. And, even though it runs much more, it has the same matte surface! As long as it is applied at normal thickness, the extra melt fluidity does not cause any running. And it has another benefit: Less cutlery marking issues. It is actually a very durable and practical food surface glaze, having a low thermal expansion that fits almost any body. Although these appear glossy here, on ware they have the identical pleasant silky matte surface.

This picture has its own page with more detail, click here to see it.
This is G2934Y (a version of the G2934 cone 6 matte base recipe that supplies much of the MgO from a frit instead of dolomite). Like the original, it has a beautiful fine silky matte surface and feels like it would not cutlery mark. But, as you can see on the left, it does! The marks can be cleaned off easily. But still, this is not ideal. The degree of matteness that a glaze has is a product of its chemistry. But can we fix this without doing any chemistry? Yes. By blending in some G2926B clear glossy (90:10 proportions). The result: The marks are gone and the surface is only slightly less matte. This underscores the need to compromise the degree of matteness, on food surfaces, enough to avoid staining and cutlery marking.

This picture has its own page with more detail, click here to see it.
These glaze cones are fired at cone 6 (without slow cooling) and have the same recipe: 20 Frit 3134, 21 EP Kaolin, 27 calcium carbonate, 32 silica. The difference: The one on the left uses dolomite instead of calcium carbonate. Notice how the MgO from the dolomite mattes the surface (without slow cooling) whereas the CaO from the calcium carbonate produces a brilliant gloss (because it needs slow cooling).

This picture has its own page with more detail, click here to see it.
Courtesy of Susan Clarke

This picture has its own page with more detail, click here to see it.
This is a buff stoneware clay. Crystal development toward a dolomite matte begins at 15%. By Kat Valenzuela.

This picture has its own page with more detail, click here to see it.
GR10-J Ravenscrag silky matte (right) and G2571A matte (left) on a dark burning iron speckled stoneware at cone 10R. The surfaces have identical feel (the chemistries are very close). The former fires a little darker color because of the iron contributed by the Ravenscrag Slip.

This picture has its own page with more detail, click here to see it.
This is G2571A cone 10R dolomite matte on an ironware body made from native North Carolina clays. Few glazes have the pleasant silky feel that this has yet are still functional. The feldspar content in the body has been tuned to establish a compromise between the warmer color that low percentages have with the higher strength that higher percentages enable. Careful porosity tests were done and recorded in an account at insight-live.com. The objective was to bring the body close to 3% absorption.

This picture has its own page with more detail, click here to see it.
By Tony Hansen

This picture has its own page with more detail, click here to see it.
GR10-G Silky magnesia matte cone 10R (Ravenscrag 100, Talc 10, Tin Oxide 4). This is a good example silky matte mechanism of high MgO. The Ravenscrag:Talc mix produces a good silky matte, the added tin appears to break the effect at the edges.

This picture has its own page with more detail, click here to see it.
This production batch of G2934 cone 6 magnesia matte glaze is firing almost glossy (upper left). Matte glaze chemistries are generally sensitive - big variations in surface character can result from small changes in firing or material chemistry/physics. This recipe relies both on high MgO and lots of Al2O3 (from high dolomite and kaolin in the recipe). A change in the frit has crossed a tipping point. But there is an amazing fix: A small addition of super fine calcined alumina (400 mesh). How small? only 1%! A small change in the frit turned it glossy so this small change has fixed it. Another factor is that greater additions of alumina (shown here are 1.5, 2.0, 2.5, and 3.0%) progressively matte it more (the slow-cool C6DHSC firing is the reason for the opacity). If the alumina was not dissolving, we would expect cutlery marking and surface staining. But neither is happening, even with additions of up to 8%, achieving stony matteness.
![]() G2934 plus 10% silica actually flows more |
![]() Cone 10R dolomite matte effect at cone 6 oxidation |
![]() Ravenscrag Slip + 10% talc = fantastic cone 10R silky matte glaze |
![]() Ravenscrag Slip based dolomite matte |
| Glossary |
Calcia Matte
Calcia matte ceramic glazes are “crystal mattes” while magnesia mattes are “microstructure mattes”. They have a smoother surface but can also have finely textured, even frosty, feathery or sugary surfaces, depending cooling and crystalliztion. |
| Glossary |
Calcination
Calcining is simply firing a ceramic material to create a powder of new physical properties. Often it is done to kill the plasticity or burn away the hydrates, carbonates, sulfates of a clay or refractory material. |
| Glossary |
Matte Glaze
Random material mixes that melt well overwhelmingly want to be glossy, creating a matte glaze that is also functional is not an easy task. |
| Glossary |
Bamboo Glaze
A high temperature reduction glaze made by adding a small amount of iron oxide to a magnesia matte base glaze |
| Glossary |
Phase Separation
Phase separation in glaze melts creates microscopic discontinuities that affect transparency, color variegation, matte surfaces, and reactive glaze effects. |
| Recipes |
G2934 - Matte Glaze Base for Cone 6
A base MgO matte glaze recipe fires to a hard utilitarian surface and has very good working properties. Blend in the glossy if it is too matte. |
| Recipes |
G2928C - Ravenscrag Silky Matte for Cone 6
Plainsman Cone 6 Ravenscrag Slip based glaze. It can be found among others at http://ravenscrag.com. |
| Properties | Glaze Matteness |
| Properties | Glaze Variegation |
| Oxides | MgO - Magnesium Oxide, Magnesia |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk