This works well on PlainsmanM340, but especially on a whiteware like M370. Produces an ivory white with some fleck. The surface is very silky, reminiscent of a cone 10 dolomite matte. Its matteness is adjustable by varying the amount of calcinedkaolin (or simply blending in a glossy recipe to shine it up a little). The mechanism of the matteness is high MgO in a boron base of low Si:Al ratio.
Do not use regular kaolin, the glaze will shrink too much during drying.
Use enough water in the slurry so it flows well, it will apply very evenly without drips. If there is not enough water and the slurry is too creamy, it will crack during drying and crawl during firing. Calcine part of the Ravenscrag to reduce the shrinkage if needed.
The tin oxide is included to whiten and opacify the glaze, if you remove it the color will be quite a bit darker, especially on darker clay bodies (Ravenscrag contains some iron). The 1.5 wollastonite is a remnant of how this glaze was created; it started as Moores Matte, a well-known Gerstley Borate-based matte recipe. We first reformulated it to substitute the GB for a frit (while maintaining the same chemistry) and then incorporated Ravenscrag Slip to supply as much of the rest of the chemistry as possible. A further adjustment was made to make the surface more silky. The silky matte G2934 followed this, it being a cleaner, whiter variant having no Ravenscrag but the same fired surface.
Since this has some iron, colouring it with stains could produce more muddied colours than you might want. Consider using the G2934 base instead if needed.
Related Information
G2928C does not work well on dark-burning bodies
This picture has its own page with more detail, click here to see it.
PlainsmanM390 (right) generates gases of decomposition (from its LOI) at a time when the G2926C glaze is unable to handle them (thus they leave pinholes and bubbles). The same glaze is good on M340 (a buff stoneware on the left), but it is even better on a porcelain.
A functional matte liner glaze is possible - with care.
This picture has its own page with more detail, click here to see it.
RavenscragG2928C matte liner glaze is on the insides of these mugs. Like our G2934 recipe, this matte glaze needs to be fired to a real cone 6 and fired in the C6DHSCdrop and hold and then slow-cooled schedule. If cooled too slowly the surface could be too matte would be subject to cutlery marking (especially on the inside bottoms). If cooled too quickly it will be too glossy. When firings cool slowly just because they are tightly packed the degree of matteness can be tuned by blending in just enough glossy glaze to make the surface smooth enough to be functional while still matte enough to be attractive to the eye and the touch.
Ravenscrag based silky MgO matte at cone 6
This picture has its own page with more detail, click here to see it.
Cone 6G2928CRavenscrag Silky Matte on PlainsmanM340 (left) and M370 (right). The inside of the M370 mug is a transparent glossy. This recipe produces a silky ivory-coloured surface of very good quality.
Comparing two glazes having different mechanisms for their matteness
This picture has its own page with more detail, click here to see it.
These are two cone 6 matte glazes (shown side by side in an account at Insight-live). G1214Z is a calcia matte, it has a high silica:alumina ratio. It crystallizes during cooling to make the matte effect. Melt fluidity is needed for that and this GLFL test shows that it certainly has that. The degree of matteness is adjustable by tuning the SiO2 content. The G2928C is a magnesia matte, it has high MgO and produces the classic silky micro-wrinkled the surface. Its matteness is adjustable by trimming the calcinedkaolin. CaO is a standard oxide that is in almost all glazes, 0.4 is not high for it. But much less MgO is needed for it to make a matte. The G2928C also has 5% tin, if that was not there it would be darker than the other one because Ravenscrag Slip has some iron. This glaze actually has texture like a dolomite matte at cone 10R, it is great. And it has wonderful application properties. And it does not craze, on PlainsmanM370 (it even survived a 300F-to-ice water IWCT test). This looks like it could be a great liner glaze.
This surprised me about calcia matte glazes:
Most are highly melt fluid.
This picture has its own page with more detail, click here to see it.
Unfortunately, many matte glazes are such simply because they are not melted enough. That is not the case with cone 6G1214Z tested here. When applied as a thin layer on pottery, it seems normal. But this GLFL test demonstrates that it fires highly melt fluid, much more than one might expect from a matte glaze. A quick look at its oxide chemistry reveals the reason: It is a calcia matte. It has high CaO, so as the melt cools, it combines with SiO2 and even Al2O3 to form calcium silicate crystals (instead of staying in the glass).
What is the G2928C? That is Ravenscrag cone 6 Tri-Matte; it employs three matteness mechanisms: High CaO, MgO and Al2O3. It contains significant Tin Oxide (thus the white color).
No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me.
XML to Paste Into Insight-live
<?xml version="1.0"?>
<recipes version="1.0" encoding="UTF-8">
<recipe name="Ravenscrag Silky Matte for Cone 6" keywords="Plainsman Cone 6 Ravenscrag Slip based glaze. It can be found among others at http://ravenscrag.com." id="119" date="2022-01-30" codenum="G2928C">
<recipelines>
<recipeline material="Ferro Frit 3134" amount="11.000"/>
<recipeline material="Talc" amount="8.000"/>
<recipeline material="Ravenscrag Slip" amount="60.000"/>
<recipeline material="Nepheline Syenite" amount="13.000"/>
<recipeline material="Wollastonite" amount="1.500"/>
<recipeline material="Calcined Kaolin" amount="12.000"/>
<recipeline material="Tin Oxide" amount="5.000" added="1"/>
<url url="https://backup.digitalfire.com/recipe/119" descrip="https://backup.digitalfire.com/recipe/119"/>
</recipelines>
<urls/>
</recipe>
</recipes>