This is an excellent alternative to the GR6-E Raspberry recipe. It is simpler, just a stain addition to the standard transparent. It is more reliable. It is easy to adjust the amount of stain to get the exact shade you want. This base recipe is unusual in that it supports the development of chrome tin stains, these are available in many shades from pink to red, consider trying a different another if this color is not right for you.
Because this is transparent (contains no opacifier), different thicknesses have different intensities of color. Because it employs a stain it will be more consistent than one using chrome and tin. Add an opacifier, like titanium, to create a more pastel color with variegation (e.g. 2-4%).
No special firing curve is needed and the surface fires very clean and defect free (with a normal soak at cone 6, or even better, the C6DHSC schedule).
For mixing instructions please see the master recipe, GR6-A.
Related Information
Ravenscrag Raspberry on porcelain
This picture has its own page with more detail, click here to see it.
Maroon and white mug before and after firing: What a difference!
This picture has its own page with more detail, click here to see it.
The outer glaze is RavenscragGR6-E Raspberry, the bright maroon color is a product of the surprising interaction between the 0.5% chrome oxide and 7.5% tin oxide present. That small amount of chrome is only enough to give the raw powder a slight greenish hue, hardly different than the clear liner glaze. While this color mechanism appears to be effective, it is delicate. A maroon stain is actually a better choice. It would fire more consistent would be less hazardous to use. And the raw glaze will be the same color as the fired one!
Cone 6 GR6-E Ravenscrag Raspberry glaze
This picture has its own page with more detail, click here to see it.
GR6-E and GR6-L Ravenscrag Pink glazes side-by-side
This picture has its own page with more detail, click here to see it.
The GR6-L (the two on the left) employs raw chrome and tin, the GR6-E uses a stain (Mason 6006). The L does not melt quite as well (because of the 10% whiting in the recipe to make sure it develops the chrome-tin color well). The GR6-E is does not need the whiting. The E is more flexible because one can choose different stains to get different colors. Of course the intensity of the color can be adjusted by varying the percentage of colorant. And the L could be made to melt better by increasing the percentage of frit.
Ravenscrag Cone 6 white glaze with 10% Mason chrome tin stain
This picture has its own page with more detail, click here to see it.
The body is PlainsmanM340 and these two glazes are based on the GR6-A recipe (Ravenscrag Slip + 20% frit). The GR6-C creamy white glaze adds 10% Zircopax to opacify it. The pink version, our code numberGR6-L, adds Mason 6006 stain instead. The GR6-A base is zinc-free and just hits the 10% minimum CaO recommended to get color development with a chrome tin stain. This recipe also couples a low MgO level (MgO can kill the color in chrome tin stains).
Ravenscrag Cone 6 Raspberry glaze on light and dark burning bodies
This picture has its own page with more detail, click here to see it.
This is GR6-LRavenscrag Raspberry glaze fired at cone 6 using the C6DHSC schedule. The body on the left is PlainsmanM340. On the right is Coffee Clay. The black burning color of the Coffee Clay is due to a 10% raw umber addition, the manganese in the umber interacts on edges where it is thinner.
A breaking glaze highlights incised decoration:
The mechanism is variation in thickness
This picture has its own page with more detail, click here to see it.
This is the Ravenscrag slip cone 6 base (GR6-A which is 80 Ravenscrag, 20 Frit 3134) with 10% Mason 6006 stain (our code GR6-L). Notice how the color is white where it thins on contours, this is called "breaking". Thus we say that this glaze "breaks to white". The development of this color needs the right chemistry in the host glaze, and it needs depth to work (on the edges the glaze is too thin so there is no color). The breaking phenomenon has many mechanisms; this is just one. Interestingly, the GR6-A transparent base has more entrained micro-bubbles than a frit-based glaze; however, these enhance the color effect in this case.
Bad and good glaze laydown:
The difference was the rheology.
This picture has its own page with more detail, click here to see it.
The problem was the rheology. The specific gravity was too high, even on a quick dip it built thickness unevenly and way too fast. And there were drips that were so big they had to be shaved off with a knife! After the addition of a lot of water, to take the specific gravity from 1.55 to 1.45 it was watery enough to accept some Epsom salts to make it thixotropic. The difference was amazing, it went on totally smooth without a single drip, producing the result on the right.
No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me.
XML to Paste Into Insight-live
<?xml version="1.0"?>
<recipes version="1.0" encoding="UTF-8">
<recipe name="Ravenscrag Cone 6 Transparent Burgundy" keywords="A stain-based method to achieve this color using the Ravenscrag base recipe." id="113" date="2024-03-17" codenum="GR6-L">
<recipelines>
<recipeline material="Ravenscrag Slip" amount="40.000"/>
<recipeline material="Ravenscrag Slip 1000F Roast" amount="40.000"/>
<recipeline material="Ferro Frit 3134" amount="20.000"/>
<recipeline material="Mason 6006 Stain" amount="10.000" added="1"/>
<url url="https://backup.digitalfire.com/recipe/113" descrip="https://backup.digitalfire.com/recipe/113"/>
</recipelines>
<urls/>
</recipe>