These add technical detail, development info, variations and improvements.
Modified: 2025-02-04 20:59:08
This glaze was born as a demonstration of how to use chemistry to convert a glossy cone 6 glaze into a matte.
| Material | Amount |
|---|---|
| Wollastonite | 27.00 |
| Ferro Frit 3124 | 36.00 |
| EPK | 20.00 |
| Silica | 5.00 |
| Calcined Kaolin | 13.00 |
| 101.00 | |
This is an adjustment to the original G1214Z recipe. The chemistry of this is the same, but the 37 raw kaolin in the original has been split to a combination of raw:calcined kaolin to reduce drying shrinkage (preventing cracking as it dries and crawling during firing). If unavailable, you can make your own calcined kaolin by roasting the powder in a container in a bisque firing.
Like G1214Z, this achieves a mat surface by incorporating a very high percentage of CaO in the chemistry. While visually appealing surfaces can be achieved, especially with slower cooling, leach testing should be done if metal oxide pigments are being used.
For 3000 grams we use 2600 water to get 1.45 specific gravity and good flow properties (no Epsom salts should be needed to gel the slurry, it is naturally thixotropic).

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. Of course, rutile could be used in place of titanium; it contains iron oxide that would enhance the development of blue. A small amount of cobalt can also be added to enhance the blue (the G2934 magnesia matte on the left, especially, will respond to that).

This picture has its own page with more detail, click here to see it.
This is the G1214Z1 calcia matte base (as opposed to the magnesia matte G2934). The clay is Plainsman M390. 5% Zircopax was added on the left (normally 10% or more is needed to get full opacity, the partially opaque effect highlight contours well). 5% tin oxide was added to the one on the right (tin is a more effective, albeit expensive opacifier in oxidation). The PLC6DS firing schedule was used.

This picture has its own page with more detail, click here to see it.
Double-layered on top half. Fired with the PLC6DS schedule.

This picture has its own page with more detail, click here to see it.
The glaze is G1214Z1 cone 6 base calcia matte on Plainsman M390 fired at cone 6 using the PLC6DS schedule. 5% titanium dioxide has been added (a high percentage). Titanium can create reactive glazes, like rutile, with no other colorants added. This effect also works well on matte surfaces, but the glaze needs good melt fluidity (that is good because functional mattes melt well). Calcia mattes host crystallization and work particularly well. Because titanium dioxide does not contain iron oxide, lighter colors and better blues are possible compared to rutile (iron is still needed, but it is coming from the body here). Like rutile, the effects are dependent on the cooling rate of the firing, slower cools produce more reactivity. Even application without drips is important (mixing as a thixotropic dipping glaze is best). This appearance also depends on using a dark-burning body or engobe.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. The tin is on the right.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. These are commonly used base glazes. The top one is a magnesia matte, next down is a calcia matte. They react very differently to these additions. Notice also the difference when titanium dioxide is applied thickly. Tin oxide fires whiter than zircon (e.g. Zircopax). Each opacifier has issues. Tin is expensive. Titanium is difficult to mix into the slurry (screening required), not as white or opaque, variations in thickness produce more difference in results and it can turn blue. Zircon is more likely to cutlery mark, twice as much is required and it amplifies the color of any iron present.

This picture has its own page with more detail, click here to see it.
The reason for this rather strange-looking wrinkling, experienced by one potter, is not obvious. But I suspected the high clay percentage in the G1214Z matte base glaze recipe (which increases drying shrinkage, thus cracking, leading to crawling). I suspect these wrinkles are actually partially healed crawling cracks. The high-clay glaze shrinks and develops tiny cracks or locally loses its bond with the bisque during drying. During firing, the fluid melt begins to pull away at these fault lines, but then flows enough to heal most of them. What remains are these unusual wrinkles rather than the bare patches normally associated with crawling.
To reduce shrinkage, I supply the kaolin as a mix of raw and calcined. The original recipe called for 37 kaolin; I supplied that with 20 EPK and 15 calcined kaolin (15 is the LOI adjusted amount). For most people, the original 37 raw kaolin version is too high (unless a high solids glaze slurry is thinly applied to porous bisque). If you need to prove this, glaze identical test pieces with all-raw G1214Z and raw/calcined G1214Z1, at the same measured thickness and SG. Before firing, inspect them with a magnifier, not just when they first appear dry, but again 5-15 minutes later (high-clay coatings can continue shrinking after they look dry).

This picture has its own page with more detail, click here to see it.
These are two cone 6 matte glazes (shown side by side in an account at Insight-live). G1214Z is a calcia matte, it has a high silica:alumina ratio. It crystallizes during cooling to make the matte effect. Melt fluidity is needed for that and this GLFL test shows that it certainly has that. The degree of matteness is adjustable by tuning the SiO2 content. The G2928C is a magnesia matte, it has high MgO and produces the classic silky micro-wrinkled the surface. Its matteness is adjustable by trimming the calcined kaolin. CaO is a standard oxide that is in almost all glazes, 0.4 is not high for it. But much less MgO is needed for it to make a matte. The G2928C also has 5% tin, if that was not there it would be darker than the other one because Ravenscrag Slip has some iron. This glaze actually has texture like a dolomite matte at cone 10R, it is great. And it has wonderful application properties. And it does not craze, on Plainsman M370 (it even survived a 300F-to-ice water IWCT test). This looks like it could be a great liner glaze.

This picture has its own page with more detail, click here to see it.
True functional mattes have fluid melts, like glossy glazes. They need this in order to develop a hard, non-scratching, durable glass. The mechanism of the G1214Z1 matte on the right is high Al2O3, it is actually melting more than the glossy G1214W on the left (this was fired between cone 5 and 6, it normally runs right off the runway).

This picture has its own page with more detail, click here to see it.
Stains can work surprisingly well in matte base glazes like the DIY G2934 recipe. The glass is less transparent and so varying thicknesses do not produce as much variation in tint as glossy bases do. Notice how low many of the stain percentages are here, yet most of the colors are bright. We tested 6600, 6350, 6300, 6021 and 6404 overnight in lemon juice, they all passed leach-free. The 6385 is an error, it should be purple (that being said, do not use it, it is ugly in this base). And chrome-tin pink and maroon stains do not develop the color (e.g. 6006). But our G1214Z1 CaO-matte comes to the rescue, it both works better with some stains and has a more crystal matte surface. The degree-of-matteness of both can be tuned by cooling speed and blending in some G2926B glossy base. You can mix any of these into a brushing glaze or a dipping glaze. Be sure to blender mix them to break up any agglomerates.

This picture has its own page with more detail, click here to see it.
The body is Plainsman M390. Firing is the cone 6 PLC6DS schedule. Each horizontal row is a commonly-used base glaze. The top one is a magnesia matte, the next one down is a calcia matte, row 3 is G2926B glossy and row 4 is Ravenscrag Slip+frit. The two mattes behave very differently from each other with the additions of opacifier. Thickly applying an opacified glaze will obviously affect visual character (column 4). Tin oxide fires whiter than zircon (e.g. Zircopax). If you like the G2934 recipe, consider the G2934Y variant for better melting.

This picture has its own page with more detail, click here to see it.
These pieces were made from Plainsman Polar Ice and fired to cone 6 using variations on the PLC6DS and C6DHSC schedules. The dipping glaze is G2934Y, a recipe variant of G2934 having a finer micro-surface texture (it has the same chemistry but the MgO is sourced from a frit and talc instead of dolomite). These mugs display how well the recipe works with stains and the varying degrees of matteness we can achieve by varying the cooling rate and the percentage of glossy G2926B base blended in. As a magnesia matte, this glaze can have a surface that pleasant to the touch. It fires durable, can be quite matte without cutlery marking, and it has very good slurry and application properties (as a dipping glaze). It has a very low thermal expansion (won’t craze). It works really well with stains (except purples). It melts even better than the glossy!

This picture has its own page with more detail, click here to see it.
Unfortunately, many matte glazes are such simply because they are not melted enough. That is not the case with cone 6 G1214Z tested here. When applied as a thin layer on pottery, it seems normal. But this GLFL test demonstrates that it fires highly melt fluid, much more than one might expect from a matte glaze. A quick look at its oxide chemistry reveals the reason: It is a calcia matte. It has high CaO, so as the melt cools, it combines with SiO2 and even Al2O3 to form calcium silicate crystals (instead of staying in the glass).
What is the G2928C? That is Ravenscrag cone 6 Tri-Matte; it employs three matteness mechanisms: High CaO, MgO and Al2O3. It contains significant Tin Oxide (thus the white color).

This picture has its own page with more detail, click here to see it.
G1214Z1 is a cone 6 calcia matte glaze, it has very high melt fluidity, enabling a fine-grained crystalline matte surface to develop during cooling. A potter was steered to this recipe after finding that G2934 magnesia matte fired too variegated when stained blue. However, this failed a leaching test. So, she simply increased the SiO2 in the formula (as shown in this Insight-live screenshot of doing the chemistry). SiO2 is the glass that makes up the lion's share of all glazes, but in mattes it is minimized in favor of Al2O3 (which often comes at a cost of susceptibility to leaching). The new recipe passed the GLLE test for leaching and even enabled reducing the cobalt percentage! Notice there is a cost: She had to compromise the degree of matteness somewhat to get the more durable product (the Si:Al ratio is a factor in the degree of matteness).

This picture has its own page with more detail, click here to see it.
1214Z over Ravenscrag slip at cone 6 gives mottled surface

This picture has its own page with more detail, click here to see it.
G1214Z golden glaze sample from Lilly Ann Hume

This picture has its own page with more detail, click here to see it.
G1214Z blue glaze from Lilly Ann Hume
| Articles |
G1214M Cone 5-7 20x5 glossy transparent glaze
This is a base transparent glaze recipe developed for cone 6. It is known as the 20x5 or 20 by 5 recipe. It is a simple 5 material at 20% each mix and it makes a good home base from which to rationalize adjustments. |
| Articles | The Right Chemistry for a Cone 6 Magnesia Matte |
| Articles |
Reducing the Firing Temperature of a Glaze From Cone 10 to 6
Moving a cone 10 high temperature glaze down to cone 5-6 can require major surgery on the recipe or the transplantation of the color and surface mechanisms into a similar cone 6 base glaze. |
| Articles |
G1214Z Cone 6 matte glaze
This glaze was developed using the 1214W glossy as a starting point. This article overviews the types of matte glazes and rationalizes the method used to make this one. |
| Articles |
G1214W Cone 6 transparent glaze
The process we used to improve the 20x5 base cone 6 glaze recipe to produce G1214W. |
| Recipes |
G1216M - Cone 6 Ultraclear Glaze for Porcelains
Substitute for low expansion cone 6 G1215U, this sources MgO from talc instead of a frit |
| Recipes |
G2928C - Ravenscrag Silky Matte for Cone 6
Plainsman Cone 6 Ravenscrag Slip based glaze. It can be found among others at http://ravenscrag.com. |
| Recipes |
G2934 - Matte Glaze Base for Cone 6
A base MgO matte glaze recipe fires to a hard utilitarian surface and has very good working properties. Blend in the glossy if it is too matte. |
| Recipes |
G1214M - 20x5 Cone 6 Base Glossy Glaze
Developed by Tony Hansen in the 1980s. Its was popular for the simplicity and how well it worked with chrome-tin stains. |
| Typecodes |
Medium Temperature Glaze Recipes
Normally fired at cone 5-7 in electric kilns. |
| Typecodes |
Matte Glaze Recipes
Much less common that glossy glazes, normally have stricter firing requirements. |
| Typecodes |
INSIGHT Glaze Recipes
These are sample recipes included with INSIGHT software. |
| Firing Schedules |
Plainsman Cone 6 Electric Standard
Used in the Plainsman lab to fire clay test bars in our small kilns |
| Glossary |
Matte Glaze
Random material mixes that melt well overwhelmingly want to be glossy, creating a matte glaze that is also functional is not an easy task. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
<?xml version="1.0"?> <recipes version="1.0" encoding="UTF-8"> <recipe name="Cone 6 Calcium Matte v2" keywords="This glaze was born as a demonstration of how to use chemistry to convert a glossy cone 6 glaze into a matte." id="3" date="2025-02-04" codenum="G1214Z1"> <recipelines> <recipeline material="Wollastonite" amount="27.000"/> <recipeline material="Ferro Frit 3124" amount="36.000"/> <recipeline material="EPK" amount="20.000"/> <recipeline material="Silica" amount="5.000"/> <recipeline material="Calcined Kaolin" amount="13.000"/> <url url="https://backup.digitalfire.com/recipe/3" descrip="https://backup.digitalfire.com/recipe/3"/> </recipelines> <urls/> </recipe> </recipes>
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk