Description: Zirconium Silicate
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| ZrO2 | 67.21% | 1.00 | |
| SiO2 | 32.79% | 1.00 | |
| Oxide Weight | 183.34 | ||
| Formula Weight | 183.34 | ||
Zircopax is a brand name of zirconium silicate (or zircon). It is primarily used in ceramics to opacify glazes. In North America, the most popular zirconium opacifiers fall under the brand names of Zircopax Plus, Superpax, Zircosil and Excelopax. These vary according to particle size, the finer the size the greater the scattering of light (and thus the better the opacification). In addition, the finer-sized materials contain a little extra silica for maximum whiteness.
Of course, the amount of zircopax in a glaze determines the opacity. Small amounts (1-3%) may give no noticeable difference but are sometimes employed to improve glaze hardness. Since zircopax is refractory, the more that is added the more the degree of glaze melting (and melt viscosity) is going to be affected. Up to 15% or more might be needed to fully opacify a glaze. If higher amounts are needed the glaze formulation may need to be adjusted to reduce the amount of SiO2 or increase flux (to melt the glaze better).
Zircopax affects glaze melt viscosity, surface smoothness, thermal expansion and color development and can be implicated in a range of glazes faults associated with these. Please read the page on zircon for more information.
Zirconium prices are have increased rapidly in recent years, reflecting the world supply situation. Even though the material is very expensive, Zircopax is added to the body recipe of “porcellanato” tiles. It is a very effective body whitener, especially for casting porcelain. Excessive additions give the porcelain an artificial "white plastic" appearance.
Typical Properties:
Formula: ZrSio4 Weight: 183.1
Linear Coefficient of Expansion (25-700C cm/cm/degreeC): 42 x 10 -7
Specific gravity: 4.5
Particle Size: Zircopax Superpax Excelopax
Microns, Ave. 1.3 .74 .55
Bulk density lbs/cu ft 100 75 75
Surface area, m2/g 4.5 9.8 12.8

This picture has its own page with more detail, click here to see it.
On the left: G2571A dolomite matte fired at cone 10R. Right: 10% Zircopax has been added. Both are on a buff stoneware (H550 from Plainsman Clays).

This picture has its own page with more detail, click here to see it.
Only 3% Veegum will plasticize Zircopax (zirconium silicate) enough that you can form anything you want. It is even more responsive to plasticizers than calcined alumina is and it dries very dense and shrinkage is quite low. Zircon is very refractory (has a very high melting temperature) and has low thermal expansion, so it is useful for making many things (the low thermal expansion however does not necessarily mean it can withstand thermal shock well). Of course you will have to have a kiln capable of much higher temperatures than are typical for pottery or porcelain to sinter it well.

This picture has its own page with more detail, click here to see it.
Right: Ravenscrag GR6-A transparent base glaze. Left: It has been opacified (turned opaque) by adding 10% Zircopax. This opacification mechanism can be transplanted into almost any transparent glaze. It can also be employed in colored transparents, it will convert their coloration to a pastel shade, lightening it. Zircon works well in oxidation and reduction. Tin oxide is another opacifier, it is much more expensive and only works in oxidation firing.

This picture has its own page with more detail, click here to see it.
On Plainsman H443 iron stoneware in reduction firing. Notice Tin does not work. Also notice that between 7.5 and 10% Zircopax provides as much opacity as does 15% (Zircon is very expensive).

This picture has its own page with more detail, click here to see it.
This is G2934 cone 6 matte (left) with 10% zircon (center), 4% tin oxide (right). Although the base unopacified recipe does not cutlery mark the other two do. Although the marks clean off all of the two on the right, the zircon version (in this case Zircopax) version has the worst and is difficult to clean. Thus, a small change is all that is likely needed. One solution is to reduce the matteness of this glaze, moving to more toward a satin surface. A way to do this is to line-blend in a glossy glaze to create a compromise between the most matteness possible yet a surface that does not mark or stain. Another option is to switch to 400 mesh silica in the recipe, that will enable many more of the particles to go into solution in the melt, thus increasing the gloss a little (an improving the firing surface in other ways).

This picture has its own page with more detail, click here to see it.
These crucibles are thrown from a mixture of 97% Zircopax (zirconium silicate) and 3% Veegum T. The consistency of the material is good for rolling and making tiles but is not quite plastic enough to throw very thin (so I would try 4% Veegum next time). It takes alot of time to dewater on a plaster bat. But, these are like nothing I could make from any other material. They are incredibly refractory (fired to cone 10 they look like bisqued porcelain). However I have had mixed results for thermal shock resistance.

This picture has its own page with more detail, click here to see it.
This GLFL test for melt flow demonstrates how zircon opacifies but also stiffens a glaze melt at cone 6. Zircon also hardens many glazes, even if used in smaller amounts than will opacify.

This picture has its own page with more detail, click here to see it.
Even commercial dinnerware can suffer cutlery marking problems. This is a glossy glaze, yet has a severe case of this issue. Why? Likely the zircon opacifier grains are protruding from the surface and abrading metal that comes into contact with it.

This picture has its own page with more detail, click here to see it.
An example of crawling in a zircon-opacified glaze on a tile. The immediate source of the problem is likely at the decoration stage. The water from the blue overglaze is rewetting the white underglaze, expanding and reshrinking it. This compromises the white glaze's bond with the body, resulting in cracking and lifting of the edges of the cracks. A number of things can be done to improve the situation: Adding a binder to the white glaze, reducing the clay content or using less plastic clays in its recipe, reducing the water content of the overglaze, heating the tiles before glazing and/or decorating so they dry faster and reducing the surface tension of the glaze melt.

This picture has its own page with more detail, click here to see it.
This melt fluidity tester compares two different tin oxides in a cone 6 transparent glaze (G2926B). Opacifiers affect not just opacity in glazes, but also liquid properties of the melt. The length, surface character, opacity and color of these flows provide an excellent indication of how similar the two materials are. This is the GLFL test.

This picture has its own page with more detail, click here to see it.
It is 5 mm thick (compared to the 17mm of the cordierite one). It weighs 650 grams (vs. 1700 grams). It will perform at any temperature that my test kiln can do, and far in excess of that. It is made from a body I slurry up (80% Zircopax Plus, 16.5% 60-80 Molochite grog, 3.5% Veegum T). The body is plastic and easy to roll and had 4.2% drying shrinkage at 15.3% water. The shelf warped slightly during drying (I should have dried it between sheets of plasterboard). Firing at cone 4 yielded a shrinkage of 1%. Notice that cone on the shelf: It has not stuck even though no kiln wash was used! Zircopax is super refractory! This is sinter bonded, so the higher the temperature you can fire the stronger it will be. Although it would be very hard to make full 18 or 22-inch shelves for larger kilns, smaller ones designed to "network" would enable a tighter load of ware with a much lower shelf-to-ware weight ratio (especially using my own lightweight posts). Like alumina, this does not have the thermal shock resistance of cordierite, uneven heating can crack these.

This picture has its own page with more detail, click here to see it.
If you are interested in the most functional possible surface, consider a 2% zircon addition to your transparent glaze recipe (the outside glaze on these mugs is a copper blue, but that is not the one we are interested in). The clear glaze on the insides of these two identical cone 6 porcelain mugs has 3% and 2% zircon added. It is not being added to opacify, it is being added to toughen the surface and reduce the thermal expansion. The presence of the 2% zircon has not affected the gloss or transparency of the glaze on the right. However, the 3% on the left has opacified it just slightly and made the surface a little silky. So that is too much for this glaze (although it might be OK if the melt fluidity was higher).

This picture has its own page with more detail, click here to see it.
The cone 03 porcelain cup on the left has 10% Cerdec encapsulated stain 239416 in the G2931K clear base (this is not an underglaze with a transparent over it). The surface is badly orange-peeled because the glass is full of micro-bubbles that developed during the firing. Notice that the insides of the cups are crystal-clear, no bubbles. So here, they are a direct product of the presence of the stain. The glaze on the right has even more stain, 15%. Why isn't it even worse? It also has a 3% addition of Zircopax (zircon), which acts as a fining agent. As you can see, this makes a dramatic difference. Suppliers of encapsulated stains even recommend a zircon addition, but are often unclear about why. This is the reason.
The yellow on the right could be improved further with a slow-cool or drop-and-hold firing. And if the glaze was reformulated to use a later melting frit (so fewer bubbles even get trapped).

This picture has its own page with more detail, click here to see it.
This is the G1214Z1 calcia matte base (as opposed to the magnesia matte G2934). The clay is Plainsman M390. 5% Zircopax was added on the left (normally 10% or more is needed to get full opacity, the partially opaque effect highlight contours well). 5% tin oxide was added to the one on the right (tin is a more effective, albeit expensive opacifier in oxidation). The PLC6DS firing schedule was used.

This picture has its own page with more detail, click here to see it.
Left: An example of G2571A cone 10R magnesia matte. Right: with 10% added zircopax (zirconium silicate). The zircopax version is a very bright pasty white compared to the original.

This picture has its own page with more detail, click here to see it.
Although this is a whiteware body (Plainsman M370), under the transparent liner glaze (G2926B) the color appears ivory, off-white. But with 8% added Zircopax the quality of the color is transformed into a white that is even better than what a much more expensive New Zealand or Grolleg kaolin porcelain would exhibit with a transparent cover glaze. The outer glaze is G2934Y matte with a yellow stain. The glazes were applied inside and outside by pouring and dipping (it would not be possible to apply the yellow evenly enough by brushing).
| Materials |
Tin Oxide
Its principle use in ceramics is as an opacifier in glazes. It is very expensive. |
| Materials |
Zirconium Dioxide
|
| Materials |
Magnesium Zirconium Silicate
|
| Materials |
Zircon
Zircon (zirconium silicate) is a hard, dense, refractory ceramic material used to opacify pottery glazes and in refractory products such as kiln washes, crucibl |
| Materials |
Zircopax Plus
|
| Materials |
Zircosil
|
| Glossary |
Opacity
Opacity of ceramics glazes is normally achieved by adding an opacifier like tin oxide or zircon. However, there are chemical profiles that can turn transparent glazes milky and make it cheaper to opacify them. |
| Hazards |
Zirconium Compounds Toxicity
|
| Typecodes |
Opacifier
Opacifiers are powders that turn transparent glazes opaque by various chemical and physical mechanisms (and combinations of mechanisms). |
| URLs |
http://en.wikipedia.org/wiki/Zirconium
Zirconium at Wikipedia |
| Frit Softening Point | 2550C |
|---|
| Glaze Opacifier | Zirconium silicates are used primarily as opacifiers in glazes at all temperatures. Although tin oxide is more effective, zirconium materials are much cheaper and are more stable in reduction and less reactive with some colorants (i.e. chrome). Although zirconium oxide is effective as an opacifier, zirconium silicates disperse better and are cheaper where the glaze can tolerate or be reformulated to tolerate the added silica. |
|---|
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |