0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Limit Recipe

"Recipe logic" is the ability to sanity-check ceramic glaze recipes on sight, by noting that materials present and their relative percentages.

Key phrases linking here: unbalanced recipes, unbalanced recipe, balanced recipes, balanced recipe, recipe limits, limit recipes, sanity-checks, limit recipe, sanity check, recipe logic, sanity-check - Learn more

Details

A "limit recipe" is a sanity check. It is "recipe logic". The concept in ceramics applies to recipes of glazes, engobes, underglazes and to clay body recipes and casting slip recipes. This page deals with glazes.

There is a proliferation of pottery glaze recipes online, many of which just don’t work for functional ware. Or which impact the safety, strength and quality of your ware. Admittedly, many recipes have accompanying warnings against their use on functional ware. Or notes that they are intended for use as an over-spray to enhance the surface of an existing glaze. However, potters and hobbyists often just want to get the surface they see in a picture!

Photo not found
or not published

There are some simple sanity checks, things to know that enable identifying obvious issues, especially potential toxicity and crazing. Remember, these limits are for functional glazes, ones whose surface will touch food and that are expected to be durable. If you want to dive deeper, consider also the matter of balanced chemistry.

The concept of a limit recipe is akin to a limit formula (except it is applied on the physical material level rather than on the oxide chemistry). We expect the percentages of material types to fall within certain ranges for typical glossy and matte functional or service glazes. If they are not, red flags should pop up! Consider some examples:

Dipping glazes need clay to suspend the slurry and harden them on drying. The ideal is 15-20% kaolin or ball clay. This assumes the brands typically used in glazes, e.g. EPK or No. 5 Glaze in North America. Highly plastic clays can do the job at a lower percentage; non-plastic ones require more. Other clays are also used (and clay-like materials like Gerstley Borate). Where clay is lacking, it is common to augment with bentonite, up to 5%. Where more clay is needed (e.g. to supply Al2O3 for a matte), some calcined or roasted clay can be used to keep the raw clay material less than 25%. If the percentage of clay is too high or the type of clay is too plastic, cracking and peeling of the dried layer will result. For brushing glazes having CMC gum additions, lower clay content can be tolerated.

Photo not found
or not published

SiO2 is the building block of all glazes. Most combinations of materials do not supply enough, so most recipes contain silica. 10-30% is normal. If there is none the glaze will likely over-melt and craze. If there is 40% it won’t melt enough.

Middle and low-temperature glazes need significant boron (B2O3) to melt them. It comes from Gerstley borate and frits. What if a glaze has none of these? How will it melt sufficiently? Perhaps it employs zinc or lithium as melters. But these are troublesome. Are you ready for that? The Gerstley Borate (GB) deposit is exhausted as of 2022; it is no more, so there is no point putting effort into glazes containing it. It also presents serious issues in slurry usability and should be avoided anyway. There are GB substitutes that likely use Ulexite or Colemanite, and they may or may not work, but frits are superior. There are lots of pages on this site about how to source boron from a frit instead.

It is very common to see high feldspar percentages (up to 80%) in stoneware glazes. 30% is normal, 50% is not. There are very few circumstances in which excessive feldspar does not produce crazing.

Does a recipe contain “borax frit”? That is like a cake recipe containing “a grain flour”. Which one? There are hundreds of borax frits; they serve temperature ranges from cone 010 to 10. Which one? Some contain 2% B2O3, others 30%. The other 98% or 70% could be anything.

Photo not found
or not published

Does it contain a feldspar you don't have? Is the chemistry available, or is it at least known if it is a potash or soda feldspar so that you could substitute it for another of the same type? Specific kaolins and ball clays are known to work well in glazes; consider using them instead of those listed.

Does it contain materials you have never heard of or used? Is there information there to explain their purpose? Does it contain significant bone ash? Bone ash is a phosphate, generally used for non-functional pigmented surfaces. It is not typical in glazes and not well studied or understood, especially for functional ware.

It is normal to see 1% cobalt, it is a powerful colorant. And super expensive. But if there is 5%, that is crazy for functional ware; it is a leaching hazard. 3% copper oxide is normal; 10% is not. Copper is specifically known to reduce the leaching resistance of glazes, even 5% should trigger leach testing. Carbonate colors (like copper, cobalt) are trouble; they gas during firing and produce blisters (the oxide forms are better). Stains are better yet.

Does it contain titanium dioxide or rutile? These are used to variegate surfaces, and it is normal to see up to about 5%, but this is a tipping point. In excess of this will often cause heavy crystallization on the surface, inducing issues with cutlery marking and staining.

Barium carbonate at 5% might be OK, but 20% is very likely to produce a leaching glaze. Yet many glazes have 30%. Lithium carbonate likewise.

High percentages of calcium carbonate or dolomite? They gas like mad; can you source CaO and MgO from wollastonite and talc instead?

Are you going to do multi-layering? You cannot just take any recipe found online and expect it to be suitable for multi-layering or as a first-coat dipping glaze.

Another aspect where recipe logic applies is the practice of having a dozen, or dozens, of completely different recipes in your operation. Learn from what commercial glaze manufacturers do. They use base recipes, for example, a transparent one; to that they add pigments, opacifiers and variegators. They use frits and stains; they are less troublesome and safer than raw fluxing materials (like lithium carbonate, calcium carbonate, zinc oxide, strontium carbonate, barium carbonate) and raw metallic carbonates and oxides (like copper, cobalt, chrome, iron). Worry about finding ways to save money later by adjusting a working recipe.

Equipped with recipe logic, you will quickly be able to predict glazes likely to craze, leach, run, settle, crystallize, pinhole, bubble and blister. For artists, the opposite can also be true; they often seek these effects as part of an aesthetic.

Related Information

Glaze recipes online waiting for a victim to try them!


A pile of printed recipes to try, but few are likely to work

This picture has its own page with more detail, click here to see it.

You found some recipes. Their photos looked great, you bought $500 of materials to try them, but none worked! Why? Consider these recipes. Many have 50+% feldspar/Cornwall/nepheline (with little dolomite or talc to counteract their high thermal expansion, they will craze). Many are high in Gerstley Borate (it will turn the slurry into a bucket of jelly, cause crawling). Others waste high percentages of expensive tin, lithium and cobalt in crappy base recipes. Metal carbonates in some encourage blistering. Some melt too much and run onto the kiln shelf. Some contain almost no clay (they will settle like a rock in the bucket). A better way? Find, or develop, fritted, stable base transparent glossy and matte base recipes that fit your body, have good slurry properties, resist leaching and cutlery marking. Identify the mechanisms (colorants, opacifiers and variegators) in a recipe you want to try and transplant these into your own base (or mix of bases). And use stains for color (instead of metal oxides).

It is possible to spot a leaching glaze just by looking at it!


A matte black coffee mug with leaching glaze

This picture has its own page with more detail, click here to see it.

This glaze looks too matte, too metallic, too crystalline. This picture was sent to me by a worried person who had bought it and noticed it discolouring on the inside. The potter may very well have considered this safe just because it was fired to cone 10. It is common among potters to overload glazes with raw metal oxide blends, often 15% or more (e.g. manganese, copper, iron, nickel, cobalt). These percentages cannot be held in solution in the melt as it cools and solidifies, so they precipitate out and crystallize, especially if the glaze is not melting well or has insufficient SiO2. The crystalline forms of these metals might look nice to some people, but the glaze is likely to leach them. It is better to use a ceramic stain to create a black like this, adding it to a stable matte base glaze (one that melts well and has sufficient SiO2 and Al2O3 to create a durable glass). The concept of a limit recipe is helpful in eyeballing recipes for their likelihood of leaching.

I made the mistake many others likely do:

Missed the one short descriptive sentence


A recipe accompanied by fancy pictures that make it look credible

This picture has its own page with more detail, click here to see it.

This is an example of an online recipe at a respected source. I deal with hundreds of customer glaze issues a year, and people expect recipes to work as shown when no documentation is included (except for "combine with non-saturated glazes for rich earth tones"). And they expect it to be functional.

The first red flag: There is no silica! Running during firing is thus expected (and happening). But it also means poor durability. There is a ton of feldspar; that means a high level of sodium. Without low-expansion MgO to counterbalance its high thermal expansion, the glaze is going to craze. The mechanism of the crystallization is titanium oversupply; with triple the typical it will certainly cutlery mark and stain. Given the unbalanced chemistry, any added colorant will likely be leachable! My slow-cool firing made the surface so dry it was very unpleasant to touch. Maybe this needs fast cooling. But who knows, there are no notes. This does not appear to belong on any functional ware, inside or outside. Someone noted that people use this to produce layering effects (see links). That begs documentation on how that would work. Without gum, would it lift and crawl as layers are added over it. Would you have to overlay every square inch? Would it still craze? All the how-to information needed to make it work is more important than the recipe itself.

A high feldspar glaze is settling, running and crazing. What to do?


Blue glaze with chemistry calculations

This picture has its own page with more detail, click here to see it.

The original cone 6 recipe, WCB, fires to a beautiful brilliant deep blue green (shown in column 2 of this Insight-live screen-shot). But it is crazing and settling badly in the bucket. The crazing is because of high KNaO (potassium and sodium from the high feldspar). The settling is because there is almost no clay in the recipe. Adjustment 1 (column 3 in the picture) eliminates the feldspar and sources Al2O3 from kaolin and KNaO from Frit 3110 (preserving the glaze's chemistry). To make that happen the amounts of other materials had to be juggled. But the fired test revealed that this one, although very similar, is melting more (because the frit releases its oxides more readily than feldspar). Adjustment 2 (column 4) proposes a 10-part silica addition. SiO2 is the glass former, the more a glaze will accept without losing the intended visual character, the better. The result is less running and more durability and resistance to leaching.

Start glaze chemistry by learning when you don't need it!

A high feldspar glaze is a good example


A runny, amber, crazed glaze

This picture has its own page with more detail, click here to see it.

This reduction celadon is crazing badly. Why? Its chemistry is dominated by feldspar, which supplies lots of K2O and Na2O fluxes. Scores of recipes being traded online contain 50% or more feldspar; they benefit from these powerful fluxes but inherit their high thermal expansion (COE). Many work only because the body happens to have sufficiently high expansion - often aided by significant residual quartz.

Crazing is more than a cosmetic problem in functional pieces. It reduces ware strength and durability, can compromise food safety and turn into a customer complaint. Let's fix it, starting without chemistry:

The LOI of Gerstley Borate is a big deal

Here is how much it can affect a glaze


This picture has its own page with more detail, click here to see it.

Fired at cone 6. The samples on the bottom tiles are from ten-gram balls that have melted down (in our GBMF test). These glazes have the same chemistry, but the one of the left sources its B2O3 from Gerstley Borate (which has a high LOI). The one on the right gets it from a frit. Because the fritted version has less gases of decomposition to expel, the glass is much smoother. Curiously, the fritted version is flowing less and the red color has been lost. Why? This could be because the Al2O3, which stabilizes glazes against excessive fluidity, is being dissolved into the melt better and thus is more available for glass building.

The traffic in glaze recipes may burn your success!


The glaze dragon will burn you!

This picture has its own page with more detail, click here to see it.

Do you mix your own recipes? That's great, but the right approach to DIY is important. Online recipes might look great on a fancy website, but what are the chances they will actually fire the way they look in the picture? Or work in your circumstances? Did the contributor know the mechanism or give any sort of directions or cautions? After trying many glazes you may think you have found one that works. But does it really? How does it hold up to limit recipes? Does it have a balanced chemistry? Is it erratic and unreliable in firing? Difficult to use? Does it leach or craze or shiver or pinhole or blister? Or make you endure other problems? Be critical and cautious about foreign recipes. Most often it is better to find a base recipe, adjust and perfect it to your clay body, then add colorants, opacifiers and variegators.

We fight the dragon that others do not see


This picture has its own page with more detail, click here to see it.

There are thousands of ceramic glaze recipes floating around the internet. People dream of finding that perfect one, but they often only think about the visual appearance, not of the usability, function, safety, cost or materials. That resistance to understanding your materials and glazes and learning to take control is what we personify as the dragon. Using the resources on this site you could be fixing, adjusting, testing, formulating your own glaze recipes. Start with your own account at insight-live.com.

Inbound Photo Links


A melt flow tester showing how a normal glazes runs when melting compared to this one
The first of 15 "Fool-Proof Recipes": Wrecked my kiln shelf!

A matte glaze melt flow that is not moving at all
Before spending time trying online recipes, take a minute to do a sanity check on them


EU Food Contact testing limits are changing - 2021


High feldspar glazes craze on functional: Don't put up with it. Fix them.

A purple pottery glaze that shivers
Sanity checking a cone 6 purple pottery glaze

Val's Turpquoise glaze chemistry
Feeling good about the glazes we use on functional surfaces

Links

Glossary Limit Formula
A way of establishing guideline for each oxide in the chemistry for different ceramic glaze types. Understanding the roles of each oxide and the limits of this approach are a key to effectively using these guidelines.
Glossary Triaxial Glaze Blending
In ceramics many technicians develop and adjust glazes by blending two, three or even four l materials or glazes together to obtain new effects
Glossary Dipping Glaze
In traditional ceramics and pottery dipping glazes can be of two main types: For single layer and for application of other layers overtop. Understanding the difference is important.
Glossary Food Safe
Be skeptical of claims of food safety from potters who cannot explain or demonstrate why. Investigate the basis of manufacturer claims and labelling and the actual use to which their products are put.
Glossary Mechanism
Identifying the mechanism of a ceramic glaze recipe is the key to moving adjusting it, fixing it, reverse engineering it, even avoiding it!
Glossary Frit
Frits are used in ceramic glazes for a wide range of reasons. They are man-made glass powders of controlled chemistry with many advantages over raw materials.
Glossary Glaze Recipes
Stop! Think! Do not get addicted to the trafficking in online glaze recipes. Learn to make your own or adjust/adapt/fix what you find online.
Glossary LOI
Loss on Ignition is a number that appears on the data sheets of ceramic materials. It refers to the amount of weight the material loses as it decomposes to release water vapor and various gases during firing.
Glossary Ceramic Stain
Ceramic stains are engineered crystalline pigment powders. They are used as an alternative to employing metal oxide and have many advantages.
Glossary Brushing Glaze
Hobbyists and increasing numbers of potters use commercial paint-on glazes. It's convenient, there are lots of visual effects. There are also issues compared to dipping glazes. You can also make your own.
Articles Glaze Recipes: Formulate and Make Your Own Instead
The only way you will ever get the glaze you really need is to formulate your own. The longer you stay on the glaze recipe treadmill the more time you waste.
Articles Trafficking in Glaze Recipes
The trade is glaze recipes has spawned generations of potters going up blind alleys trying recipes that don't work and living with ones that are much more trouble than they are worth. It is time to leave this behind and take control.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy