0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Glaze Compression

In ceramics, glazes are under compression when they have a lower thermal expansion than the body. A little compression strengthens ware, too much can weaken and even fracture it.

Key phrases linking here: glaze compression, time bombs, time bomb - Learn more

Details

Every solid has a coefficient of thermal expansion (COE), that is, an amount by which it expands and contracts on heating and cooling. COE is measured in thousandths of an inch but differences in body and glaze are significant because both are rigid and inseparable. If the thermal expansion of a glaze is excessive more than the body it is affixed to, to relieve the tension of being 'stretched on' it crazes (tiny cracks in the glaze). However, when the COE is significantly lower than the body the glaze can find itself under expressive compression. This condition is most commonly evident by shivering (flaking off on convex contours). But when a glaze is applied thick enough on convex surfaces it can fracture a piece.

Photo not found
or not published

This condition can be mistaken as dunting, but the two are completely different. This is caused by a thermal expansion mismatch between body and glaze, dunting occurs when thermal gradients are introduced as pieces cool too quickly in the firing (through quartz inversion they are unable to the differing thermal expansions of each).

A worst-case scenario for glaze compression is ware having a thickly-applied low-expansion glaze on the inside with a crazing glaze on the outside. Powerful internal stresses seek an opportunity for relief and the craze line cracks on the outside provide initiation points to almost assure failure - in vitreous or non-vitreous bodies. In severe cases, pieces will not survive cooling in the kiln without fracturing (individual shards of such pieces can explode into dozens of tinier pieces upon an impact). This type of failure is also very common in ware that is not glazed on the outside. In less severe cases, pieces can fail during use (e.g. when a hot liquid is poured in). In mild cases, ware is simply weaker or more brittle than it otherwise would be.

Although glaze fit can happen by accident it is better by design. The thermal expansion of glazes is a product of their chemistry and that is the ideal level on which to approach this challenge. At a minimum, looking at the oxide chemistry can give direction on how to adjust recipes for better fit. That being said, in industry it is common for technicians to take a material-level approach to achieving glaze fit, simply trading a percentage of lower expansion frit for one having a higher expansion. However, this approach often introduces unintended side effects (because frits having complex chemistries are being treated as just expansion-adjusters). For potters there is also a viable non-chemistry approach: Where two base glazes are known to work, a blend of one having a higher-than-needed COE with one having a lower-than-needed COE could achieve the desired fit. When opacifiers and stain additions affect COE the blend can also be adjusted to compensate. Potters are also the most flexible to delve into the chemistry, the prime origin of the fired properties of glazes. Using an account at Insight-live.com one can see the calculated thermal expansion glaze recipes. By placing recipes side-by-side (e.g. an original and an adjustment) one can observe changes in the expansion as ingredients are adjusted.

Related Information

This crack is "spring loaded" out of the kiln. Why?


Low temperature cracked mug

This picture has its own page with more detail, click here to see it.

It is possible for glazes to be under a condition called "glaze compression". This is L4410P, a low-temperature dolomite body, formulated to have the highest thermal expansion possible without the use of talc. This inside transparent glaze is G3879C (we made this as a brushing glaze, four coats are needed on this body). That glaze was formulated to have the lowest expansion possible (given frits we have). As the kiln cooled the body was unable to withstand the increasing compressive forces of the solidifying glaze inside, resulting in what you see here. In the days following the firing, it kept widening, branching and travelling until the mug spontaneously split in two. Another identical mug with Spectrum 700 clear inside (same outside glaze) bounced like a ball when dropped onto concrete from two feet (a subsequent ricochet right onto the handle took off a chip). But when I dropped this one the pent-up stresses within exploded it into dozens of pieces. Neither the body or glaze are at fault, it is their mismatch that causes this. The thicker the glaze the worse it is. If the outside glaze is also "pulling" (because of a higher thermal expansion than the body) the situation is even worse.

Why is this vitreous low fire ware cracking out of the kiln like this?


Glaze compression fractures terracotta

This picture has its own page with more detail, click here to see it.

Simply put: Glaze misfit. The glaze is under compression and it is pushing outward. That compression was created as these terra cotta pieces cooled in the kiln. After the glaze solidified, somewhere above red heat, it became a glass and began to contract. The body, to which that glaze is attached by a glass bond, had its own higher rate of contraction. The glaze has some advantages in this battle. Its thick application gives it extra power to assert its thermal expansion. The body is over-fired and has become brittle. The unglazed outsides, incised designs and varying thickness provide points of weakness where cracks can start. The body resists the relentless force from inside but the odds were stacked against it and the pieces do not even make it out of the kiln. Of course, the glaze could be applied thinner, ware could be fired lower, it could have a more even cross-section and the outsides could be glazed. All will help, but increasing the thermal expansion of the glaze (by increasing KNaO at the expense of other fluxes), is one change that would fix this issue.

Why are these vessels cracking when hot water is poured in?


This picture has its own page with more detail, click here to see it.

They are time-bombs. Why? Yes, they have even wall thickness, the glaze is not crazing and the clay is vitrified. But, they are glazed only on the inside and that is a problem here. The glaze is under some compression, that is why it does not craze. That means that it is pushing outward from the inside. Ware can be very strong under glaze compression, but only to a point. When a hot liquid is poured into containers like these the inside glaze is the first to thermally expand, creating more even compression. The porcelain is under tension already, being stretched by pressure from within. And ceramics do poorly under tension. And third: The outer surfaces have incised lines that provide irregularities for internal forces to exploit and start cracks at. It is a perfect storm waiting for hot water to trigger it. Making the pieces thicker would help. Increasing the glaze thermal expansion would help. But unglazed outsides and incised lines will always be a weakening factor.

Drip glazing and bare outsides: Deceptively difficult.


thick glaze drips on ceramic vessels

This picture has its own page with more detail, click here to see it.

What issues to these carry? Glaze fit. Do these yourself and they might end up being glaze compression demonstration pieces. These are available on Aliexpress (as Drip Pottery, Drippy Pottery or Goopy Glazes) and they are made by a manufacturer that has close control of body maturity (and thus strength) and the capability to tune the thermal expansion fit of glaze-on-body. Glaze fit has to be better than normal because of the absence of an outside glaze on much of the surface. Too low an expansion and the compression (outward pressure) will fracture body (especially for thin-walled pieces). Too high and it will craze. And if the glaze is thick, it will shiver or craze with far less forgiveness than a thin layer. And how did they get the glaze on this thick? They likely deflocculate it, up to 1.7 or more, glaze the inside, let it dry, then glaze the outside. And apply the glaze to preheated ware. If done right, these pieces are a visual and technical achievement. However, drippy glazes in the hands of hobbyists carry more risk. They often just multiple layers of commercial brushing glaze that only by accident fits the body being used. No wonder their pieces often end up as time-bombs or crazed bacteria farms.

A low temperature vase has exploded while just sitting there! Why?


This picture has its own page with more detail, click here to see it.

This is a slip-cast vase. The body is a typical 50:50 talc:ball clay blend. Only the outside of the vessel is glazed. The talc increases the thermal expansion so that during cooling in the kiln the body contracts more than the glaze, putting it under compression (and thereby preventing crazing). But, these bodies have no flux, they typically have 10%+ porosity and often are not strong enough to resist for long the tensive forces the glaze can put them under. This is especially so when walls are thin. Or when only the inside is glazed. Or when the inner glaze is under compression and the outer under tension. How could such a thing happen? When potters use glazes from one manufacturer and trust they fit bodies made by another (which is almost always).

Glaze Compression:

A mug cracks before your eyes

The glaze on this highly vitreous, thin-walled mug is normally perfect; it is under enough thermal compression to really increase ware strength. But since this mug is glazed inside only, the compression is too great. While it looks OK, the glaze is constantly pressing outward, looking for relief. Watch as a tap with a spoon is enough to trigger a sudden crack. And it opens under the pressure, clearly revealing the piece was spring-loaded. A typical mug of this clay would survive hundreds of impacts of this nature. Further, this did not happen just because it was not glazed on the outside. A mug with glaze under compression on the inside and another glaze under tension on the outside would fail this test even more dramatically.

Is inside-only glazing a good idea?

Here's an example to question that


Glaze compression fractures porcelain mug

This picture has its own page with more detail, click here to see it.

This mug is made from 325 mesh MNP, the strongest porcelain I have. Since the walls are of even thickness with no abrupt corners or contour changes and the glaze is thinly and evenly applied I thought I could follow a social-media-driven trend and glaze only on the inside. But I got glaze compression time-bombs waiting for hot coffee triggering! Three other mugs failed this same way! But four with this same glaze inside and out were fine. Why? The outside glaze counters the inside one, pushing outward. And it closes crack initiation points.

I got lots of pushback from people who said glaze compression problems are overblown. But I also have stories and pictures much worse than this (especially with thick and drippy glazes). But some still feel that inside-only glazing can work by carefully tuning the thermal expansion fit between body and glaze. Or even by accident. Either way, there is still an elephant in the room: Glaze fit has to be just right - too much and pieces break, too little and the glaze crazes. That is a problem because it brings intolerance of even small changes in body, glaze or firing.

Of course, by making thicker-walled ware, having a glaze thickness that is not excessive, you may still get away with doing everything just advised against! But think about this: This coffee could have ended up in my lap rather than on my paper?

The glaze broke the bottom off the pot!


This picture has its own page with more detail, click here to see it.

An example of a highly fluid cone 6 glaze that has pooled in the bottom of a mug (and crystallized). Glazes normally need to be under some compression to avoid crazing (by having a lower-than-the-body thermal expansion), but if they are thick like this the body does not have the strength to resist the extra outward pressure the glaze can be exerting at the base from the inside. The result here is a separated base. Conversely, if the glaze is under tension (having too high an expansion), the cracks that develop within it to relieve the tension are deep and wider and thus more likely to propagate into the body. The ultimate result: Poor ware strength and durability. A better solution is to use a liner glaze.

To gauge strength: Break pieces often. Pay attention to what happens.


A broken slip cast cone 6 mug

This picture has its own page with more detail, click here to see it.

This is M340 casting, L3798H. The handle was just glued on with slip. I had questions about this new body. Are my glazes under compression? How well is the handle stuck on? Because I have broken so many pieces I know how their fracture pattern. It is a good sign when there are no fractures along the handle joins. And when the handle is the last to go. And when the item breaks into large pieces rather than shattering into small ones. Try doing this on some of your pieces and you might be surprised. Either by how strong they are. Or by how easily they break.

Yellow stain has decreased the thermal expansion of the base glaze


This picture has its own page with more detail, click here to see it.

That has put it under more compression on the inside, it is pushing outwards. All it took was some hot coffee. That put it under even more compression and the mug "popped" to relieve the tension.

Example of COE curves considered a good fit for body and glaze


COE charts for sanitaryware glaze, body

This picture has its own page with more detail, click here to see it.

These are from a sanitaryware plant in India. Long-term glaze fit is essential for their products. The glaze thus needs to be under some compression. That means the body must have a slightly higher coefficient of thermal expansion (COE) than the glaze. These two charts were created on the same dilatometer by the same person using well-defined procedures (the glaze and clay each have their own procedures). A history of measurements and associated knowledge of how the data relates to the quality of the fired products provides a context to interpret these reports. In other words, technicians have learned that the difference shown here is what is required to achieve optimal glaze fit for this specific body/glaze combination. Of course, some sort of database system (e.g. lab notebook, an account at insight-live.com) is needed to record the history of testing to be able to effectively compare the past with the present.

A novel way to test glaze compression and glaze fit


Two coffee mugs, one cracked, the other shattered

This picture has its own page with more detail, click here to see it.

These are made from L4005D red cone 6 stoneware. Both are cast and thin-walled (half of what a thrown piece would be). They were glazed only on the inside to encourage cracking/splitting if the glaze is under excessive compression (that is, the thermal expansion of the glaze is significantly less than that of the body). And that is what happened here. The piece on the left cracked after a couple of taps with a hammer. Notice how the crack has opened. The piece is "spring-loaded" (press it together and it reopens on release). The glaze is GA6-B. The piece on the right is glazed with G1214Z1. It spontaneously blew in half, with a loud crack, a few 5 hours after exit from the kiln. On further taps with a hammer these pieces shattered into dozens of smaller ones! The white glaze is certainly under too much compression. Obviously, neither is under any danger of crazing. Is the compression too great on the dark glaze? It did not shatter the way the white one did on further taps. And, another thicker-walled piece exiting the same kiln was glazed inside and out with that glaze. It was very strong. The lesson: Glaze compression, if not too much, is good for ware strength - but pieces must be glazed both outside and inside. And, thin ware like this must have better-fitted glazes.

My clear glaze outside. Commercial white inside. But a big problem!


This picture has its own page with more detail, click here to see it.

I know my outside glaze recipe fits this terra cotta. It does not shiver on sudden heating or craze on sudden cooling. And I have a gallon so I can dip-glaze the outside and it dries perfectly in seconds. But that inside glaze? It is under too much compression, so much so that it is literally forcing the piece apart (that crack exploded onto the scene with a loud ping a day after firing). But I do not know the recipe. And I had to paint it on in three coats. The painting was difficult and it took ten minutes to dry each coat. A better way to do a cover glaze would have been to simply add 10-15% Zircon to my clear recipe (I can even adjust if the added zircon lowers its expansion too much). To apply that would have been a simple pour-in and pour-out. Or I could make my own pint-jar of brush-on by using a mix of gum solution and water (instead of pure water).

Inbound Photo Links


Shivering crazing terra cotta
Shivering on terra cotta is a red light not to ignore


An extremely runny glaze at cone 6. The runniness is manageable, it has other issues!


A glaze is pushing outward from the inside of this cup: This problem did not show up on the test tiles!

Links

Glossary Glaze Crazing
Crazed ceramic glazes have a network of cracks. Understanding the causes is the most practical way to solve it. 95% of the time the solution is to adjust the thermal expansion of the glaze.
Glossary Ceramic Glaze Defects
Ceramic glaze defects include things like pinholes, blisters, crazing, shivering, leaching, crawling, cutlery marking, clouding and color problems.
Glossary Glaze fit
In ceramics, glaze fit refers to the thermal expansion compatibility between glaze and clay body. When the fit is not good the glaze forms a crack pattern or flakes off on contours.
Glossary Thermal Expansion in Ceramic Bodies and Glazes
The co-efficient of thermal expansion of ceramic bodies and glazes determines how well they fit each other and their ability to survive sudden heating and cooling without cracking.
Glossary Calculated Thermal Expansion
Calculation of the thermal expansion of glazes is a very useful comparative glaze-fit tool. But it’s not a laboratory measurement.
Glossary Glaze shivering
Shivering is a ceramic glaze defect that results in tiny flakes of glaze peeling off edges of ceramic ware. It happens because the thermal expansion of the body is too much higher than the glaze.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 