0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Flashing

A visual effect that occurs in wood and salt firing of ceramic ware. Many potters value the effect and use special materials and firing methods to enhance it.

Key phrases linking here: flashing - Learn more

Details

Photo not found
or not published

A fired visual effect on bare clay surfaces in fuel burning kilns. Clay surfaces that have been flashed have been subjected to a thermal history of variations in flame, ash, kiln atmosphere and even imposed vapors (like salt and soda). Historical ceramics often had flashing simply as a consequence of material suitability and the nature of the fuels and firing. In recent years there has been a focus on controlled reproduction of it.

In sodium vapor firing, the reaction with the clay surface forms a very thin sodium alumino-silicate glaze. Flashing happens where this reaction is slight enough that iron and other body colorants show through rather than being covered by a full glaze. “Flashing slips” for salt and soda firing are typically formulated to stay only partially active (thus non-vitreous). It is a balance. Too refractory and flashing is weak. Too fusible and one gets a glaze instead. Slip formulations having high alumina content react best with the kiln atmosphere. For that reason a high kaolin percentage is typical (for its reaction-available Al2O3). Some pure fine alumina powder can also be employed in slip recipes (using so-called ‘reactive’ finer particle sizes). The color development is understood to happen during cooling. Matters of study include understanding kaolins: Some are known to produce better flashing than others. And better understanding the sodium reaction and when it happens, iron state changes and crystal development are invaluable.

In wood firing, flashing is mainly a surface staining and very thin glaze-forming effect. Wood ash contains fluxes (like oxides of potassium, calcium, sodium). As wood burns the ash and these volatile alkalis enter the flame stream and react with hot clay surfaces. The reaction lightly attacks the clay surface, forming a microscopic alkali-rich glass layer producing oranges, reds, greys and subtle sheens. Where ash deposition becomes heavier, flashing can turn into actual ash glaze. A large part of flashing color comes from iron already present in the clay body or slip, the alkali reaction changing how that iron appears (according to kiln atmosphere). So flashing can be seen as an iron-response to alkali vapor. Pieces facing direct flame often flash more. Like salt/soda firing, slips improve flashing. Cooling also matters as it affects iron oxidation state and crystallization.

Related Information

Flashing from wood firing

The range of possible surfaces


This picture has its own page with more detail, click here to see it.

Made by Robert Self. This is Laguna White Stoneware body fired to cone 13 in a Manabigama wood fired kiln.

Test piece to demonstrate flashing

From a Manabigama wood fired kiln


This picture has its own page with more detail, click here to see it.

From Robert Self. This firing went past cone 13. The body is Laguna Speckstone.

Intense flashing at cone 10R, courtesy of nepheline syenite tiles


Intense flashing at cone 10R

This picture has its own page with more detail, click here to see it.

This flashing method works in reduction or oxidation. It was done by bisque firing a thin nepheline syenite tile leaning against the piece. The tiles are made using a 5:95 mix of Veegum and Nepheline (or a 10:90 mix of raw bentonite and nepheline). Sodium vapours from the tile are deposited on the surface and affect it profoundly enough to influence the glaze firing. A similar effect can be had by spraying on a saltwater solution, it should work whether done prior to the bisque or the glaze firing (of course lots of testing would be required to perfect it).

Soda fired porcelain vessel

By Heather Lepp


This picture has its own page with more detail, click here to see it.

This is a small cup-sized object made from Plainsman P600 (simply composed of Tile #6 kaolin, nepheline syenite and quartz). It is valued as a product-of-the-process piece, consigned to the "kiln God" as unglazed. It exhibits carbon-trap, soda glaze deposition and flashing. The soda-vapour atmosphere of the kiln glazed one side of the vessel early enough in the firing to trap carbon under a crystal-clear glass. Often such glazes are crazed, but this one likely is not because the body contains 25% quartz, giving it a high thermal expansion. The other side of the piece exhibits tones of red, brown and yellow on the bare, vitreous porcelain surface - this is characteristic of "flashing".

Links

Glossary Salt and Soda firing
Salt firing is a process where unglazed ware is fired to high temperatures and salt is introduced to produce a vapor that glazes the ware.
Glossary Wood Firing
A method of firing pottery in a fuel burning kiln (using wood) rather than gas. Temperatures beyond cone 10 can be achieved.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy