1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Copper Carbonate Basic

Alternate Names: Cupric Carbonate, Copper (II) Carbonate, Azurite

Formula: CuCO3.Cu(OH)2, CH2Cu2O5

Notes

This form of copper carbonate is the article of commerce. What you are getting when you buy it is a mixture of theoretical copper carbonate and copper hydroxide. The chemical structure sees two Cu atoms bonding to an OH each and sharing a CO3. Data sheets might quote the amount of Cu metal in the material (rather than CuCO3 or Cu(OH)2).

Copper Carbonate has a fairly complex decomposition. The accompanying curve shows the history of weight loss as this material is fired (courtesy of Bob Hickerson, World Metal, LLC). It is interesting to compare this chart with the one for Copper Hydroxide to see the difference in the amount of weight lost, and when and how fast it occurs.

As with other metallic coloring carbonates, copper carbonate is bulkier than the oxide form, thus it tends to disperse better to give more even results. It is also more reactive chemically and thus melts better. As such, it is ideal for use in brushwork where minimal speck is required. However, it produces gases as it decomposes and these can cause pinholes, orange peeling and blisters in glazes. Also, the carbonate form contains less copper per gram, therefore colors are less intense than the oxide form.

The hydroxyl component is an important aid in dispersing the powder throughout the glaze slurry and thus avoid specks in the fired glaze.

Supplies of green copper carbonate basic often vary in color and density (darker and heavier, lighter and fluffier) reflecting variations in raw materials and manufacturing procedures. Despite variations in the physical appearance of the material, the amount of contained copper metal remains essentially constant.

The raw powder begins to melt between 1950 and 2000F. At around 1500F it gases and will discolor nearby items in the kiln.

Related Information

Copper carbonate fuming


This picture has its own page with more detail, click here to see it.

And example of how copper carbonate fumes during firing. The white sample on the left was near the copper sample, at around 1500F the fumes discolored its facing edge. These are permanent, they do not fire out but get darker with increasing temperature (this is 1950F). The kiln shelf was also discolored outward about half an inch from the copper specimen.

Black ash glaze for 20% raw metal pigments: Suitable for functional ware?


Saturated metal ash glaze

This picture has its own page with more detail, click here to see it.

This glaze is 49% Wood Ash, 24% Soda Feldspar and 27% Ball Clay. 10 copper carbonate and 10 manganese dioxide are added to that. This beautiful sculpture was made by Dan Ingersoll, aesthetically this glaze is perfect for it. But there are two red flags here. Significant manganese and copper metal fumes are certain to be generated at cone 10 (they are seriously not healthy) so anyone using this must be very careful. But there is something much more serious - this glaze is being used on functional ware. Copper is well known to destabilize other metals in the fired glass. This 10:10 combination is a perfect storm for leaching heavy metal into food and drink. This is not an argument for the use of commercial glazes, it is one for common sense application of the concept of limit recipes.

Copper Carbonate is beginning to melt. When?


This picture has its own page with more detail, click here to see it.

Copper carbonate is beginning to melt at 2000F (this same sample was fired to 1950F, while shrunk to less than half its size, it was not melting yet).

Copper carbonate powder


This picture has its own page with more detail, click here to see it.

LOI test of common materials flags copper carbonate


This picture has its own page with more detail, click here to see it.

These are pure samples (with 2% binder added) of (top left to bottom right) strontium carbonate, nepheline syenite, cobalt carbonate, manganese dioxide, bentonite (in bowl), 6 Tile kaolin, New Zealand kaolin and copper carbonate. I am firing them at 50F increments from 1500F and weighing to calculate loss on ignition for each. I want to find out at what temperature they are gassing (and potentially bubble-disrupting the glaze they are in or under). Notice how the copper is fuming and spitting black specks on the shelf, this happens right around 1500F (these stains on the shelf darkened considerably when the kiln was fired higher). Yet copper carbonate does not melt and fully decompose until much higher. No wonder it is implicated in cases of glaze blistering and bubbling.

Pure cobalt carbonate and copper carbonate at 1850F


This picture has its own page with more detail, click here to see it.

Cobalt carbonate (top) and copper carbonate (bottom). Left is the raw powder plastic-formed into a sample (with 2% veegum). Right: fired to 1850F. The CuCO3 is quickly densifying over the past 100 degrees and should begin to melt soon. It is long past the fuming stage.

2% Copper in two cone 6 transparents:

One does not bubble and orange-peel. Why?


This picture has its own page with more detail, click here to see it.

The top base glaze, G2926B, has enough melt fluidity to produce a brilliant functional gloss when used as a transparent. However, for this 2% copper carbonate addition, it has too little melt fluidity and/or too much surface tension to merge, pass and heal the entrained micro-bubbles (generated by the decomposition of the carbonate).

The lower glaze, G3806B, diversifies the fluxes (half the B2O3 in exchange for more Na2O and introduction of SrO and ZnO) and increases their total compared to Al2O3 and SiO2. The result is a more fluid cone 6 melt having lower surface tension. The mixed-oxide effect is also a factor here; the diversity itself improves the melt.

The above factors are enough to solve the problem here. But more can be done. More zinc (in exchange for KNaO) could produce later melting, especially in combination with sourcing some or all of the latter from a feldspar instead of the low-melting frit. The benefit would enable more gas escape until melt-sealing (and reduce the COE).

1% and 2% copper carbonate in a cone 6 transparent


This picture has its own page with more detail, click here to see it.

The recipe, G3806B, also contains 2.5% tin oxide. The clear base is the best we found to host the copper blue effect. It was adapted from one found online, we recalculated that to source the Al2O3 more from clay and less from feldspar (to get better slurry properties). Later work was done to try to reduce the thermal expansion of this, but successes in doing that came at a loss in blue color. The COE of this simple enough to fit many bodies without crazing, porcelains having low silica percentages are least likely to fit.

Example of a data sheet for Copper Carbonate


This picture has its own page with more detail, click here to see it.

Notice it does not quote the amount of CuCO3, just Cu metal. It also does not quote LOI percentage (weight loss on ignition, it will be more than 25%). Theoretical copper carbonate is 71.94% CuO (sourced by a mix of copper carbonate and carbonate hydroxide). CuO is 79.9% copper and 20.1% oxygen. Thus, we would expect Cu metal to be 57.5% (in a theoretical material). Since this example has impurities it is a little less, 55.8%.

Switching copper carbonate for copper oxide in a fluid glaze


This picture has its own page with more detail, click here to see it.

The top samples are 10 gram GBMF test balls melted down onto porcelain tiles at cone 6 (this is a high melt fluidity glaze). These balls demonstrate melt mobility and susceptibility to bubbling but also color (notice how washed out the color is for thin layers on the bottom two tiles). Both have the same chemistry but recipe 2 has been altered to improve slurry properties.

Left: Original recipe with high feldspar, low clay (poor suspending) using 1.75% copper carbonate.
Right: New recipe with low feldspar, higher clay (good suspending) using 1% copper oxide.

The copper oxide recipe is not bubbling any less even though copper oxide does not gas. The bubbles must be coming from the kaolin.

More copper can produce fewer bubbles!


This picture has its own page with more detail, click here to see it.

The first glaze, G2926B, is a standard functional transparent glaze with added copper. The other three are part of a project to find a copper blue (G3806B has the best color and the best compromise of flow and bubble-clearing ability).

The GLFL testers for melt flow are at the back, and the GBMF test melt-down-balls contain 1% copper carbonate. The glazed samples in front have 2% copper carbonate. But why do the recipes containing half the amount of copper have far more bubbles? Because they are thinner? Not really; in use on ware, they also have fewer bubbles. Why? A small CuO addition can change where and how bubbles nucleate and how viscous the melt is. At some point between 1% and 2%, a threshold is crossed that affects nucleation and coalescence. For example, a little copper could encourage lots of tiny bubbles to form and stay trapped, while more changes the melt chemistry enough that they coalesce and escape (or simply aren’t nucleated the same way). Phase separation could produce Cu-rich droplets that enable copper to be its own fining agent.

Copper fluxes a matte glaze at cone 6


This picture has its own page with more detail, click here to see it.

4% copper carbonate and 6% rutile have been added to G2934 cone 6 matte base. Using a green stain should prevent this. Or some B2O3 could be substituted with SiO2 (via glaze chemistry).

TGA-DTA Sample curve for Copper Carbonate


This picture has its own page with more detail, click here to see it.

Malachite diagram


This picture has its own page with more detail, click here to see it.

Links

Oxide Analysis Formula Tolerance
Troubles Orange Peel Surface
Orange peel is a defect or physical property of ceramic glazes
Troubles Glaze Pinholes, Pitting
Analyze the causes of ceramic glaze pinholing and pitting so your fix is dealing with the real issues, not a symptom.
URLs https://en.wikipedia.org/wiki/Basic_copper_carbonate
Basic Copper Carbonate at Wikipedia
Oxides CuO - Cupric Oxide
Materials Copper Oxide Red
Materials Copper Oxide Black
The purest source of CuO copper oxide pigment used in ceramic glazes.
Materials Copper Hydroxide
Materials Copper Carbonate
A source of CuO copper oxide used in ceramic glazes to produce a variety of colors (used only or with other colorants).
Temperatures Copper carbonate basic decomposes (300-330)
Temperatures Copper carbonate basic breakdown (1050-)
Hazards Copper Oxide and Carbonate
Hazards Copper Compounds Toxicology
Articles Leaching Cone 6 Glaze Case Study
An example of how we can use INSIGHT software to determine of a glaze is likely to leach
Minerals Azurite
Copper carbonate mineral
Typecodes Colorant
Metallic based materials that impart fired color to glazes and bodies.
Typecodes Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials.

Data

Frit Softening Point 500C D
Density (Specific Gravity) 3.90

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy