Alternate Names: Copper (II) Oxide, Black Copper Oxide, BCO, Cupric Oxide
Formula: CuO
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CuO | 100.00% | 1.00 | |
| Oxide Weight | 79.54 | ||
| Formula Weight | 79.54 | ||
One of the oldest colorants used by potters. It is a popular source of CuO in glazes and glass. In sufficient percentages it can be a very strong flux, in a mix of 50% Ferro borax frit 3134 it will dissolve a firebrick crucible at cone 6! It is the most stable form of oxidized copper (Cuprous oxide oxidizes to cupric oxide in normal firings).
The oxide form of copper can give a speckled color in glazes whereas the carbonate form will give a more uniform effect.
Copper normally produces green colors in amounts to 5% where it moves toward black. In reduction firing, it turns to Cu2O and gives vibrant red hues. It the glaze is fluid copper will tend to crystallize heavily. See CuO and Cu2O in the oxides database for more information.
Above 1025C copper becomes increasingly volatile and its crystalline structure breaks down. At 1325C CuO melts. This can affect the color of other glazes pieces in the kiln. Glazes containing copper can change significantly because of loss of copper. Some potters alternate between reduction and oxidation, and even put a dish filled with copper carbonate in the center of the kiln to minimize this phenomenon.
There are many workable copper ores (i.e. tenorite, cuprite). Source: American Chemet Corp., 708-948-0800 FAX 708-948-0811
See also: "Coloring Mechanism of Peach Bloom Copper Red Glazes" written by four technicians from China published in Dec 91 Bulletin of the American Ceramic Society.

This picture has its own page with more detail, click here to see it.
These metal oxides have been mixed with 50% Ferro frit 3134 and fired to cone 6 oxidation. Chrome and rutile have not melted, copper and cobalt are extremely active melters, frothing and boiling. Cobalt and copper have crystallized during cooling. Manganese has formed an iridescent glass.

This picture has its own page with more detail, click here to see it.

This picture has its own page with more detail, click here to see it.
The color red is difficult to achieve in ceramics. In reduction firing copper can turn many dazzling shades of red.

This picture has its own page with more detail, click here to see it.
Left: The base recipe of GA6-C (80% Alberta Slip, 20% Frit 3134, 4% rutile). That recipe is stable; it does not run. Right: A 2% addition of copper carbonate transforms it into a runny, melt fluid glaze. It also produces a pleasant green even on this red-burning body (a good green is not easy in oxidation ceramics). Using a catch glaze (e.g. a frit-reduced version), this could be made safe on vertical surfaces. However, there are red flags here. Having only 2% copper would not destabilize a typical glaze (making it leachable). But phase separation is occurring here, likely because the base contains significant rutile. That means the phases are copper-bearing and possibly copper-concentrating. And, as noted, the copper has a greater-than-expected impact on the melt. Third, commercial variegated copper glazes can even leach in acids (as happened with the mug inset after a night with lemon juice). While the GA6-C recipe does have a 0.3:0.7 R2O:RO ratio, other indicators make it a course of wisdom to consider the GLLE test before use on functional surfaces.

This picture has its own page with more detail, click here to see it.
The top samples are 10 gram GBMF test balls melted down onto porcelain tiles at cone 6 (this is a high melt fluidity glaze). These balls demonstrate melt mobility and susceptibility to bubbling but also color (notice how washed out the color is for thin layers on the bottom two tiles). Both have the same chemistry but recipe 2 has been altered to improve slurry properties.
Left: Original recipe with high feldspar, low clay (poor suspending) using 1.75% copper carbonate.
Right: New recipe with low feldspar, higher clay (good suspending) using 1% copper oxide.
The copper oxide recipe is not bubbling any less even though copper oxide does not gas. The bubbles must be coming from the kaolin.

This picture has its own page with more detail, click here to see it.
This G3806D fluid melt glaze recipe demonstates the different color characteristics imparted by copper carbonate (left) and copper oxide (at 2%). The carbonate version is bluer and less intense. Copper carbonate is about 65% CuO while the oxide version is 100%. Our supply of the oxide version is not producing any specking (if yours does you may need to sieve or blender mix the slurry).

This picture has its own page with more detail, click here to see it.
These are among about 150+ of the best mugs I have ever made. I have them on hand, and I have cataloged, coded, photographed from 6 angles and described every detail about how I made them. Following is the kind of description each piece has. The linked words go to the Digitalfire Reference Library for endless research on particulars.
Clay: Polar Ice Cone 6 translucent porcelain
Glaze outside: G3806 base (copper-blue variation)
Glaze inside: G2926B transparent glossy
Firing: Cone 6 C6DHSC slow cool
Size: 10cm high, 9cm dia, 280, 310ml capacity
Foot: Tooled and fluted
Technique: Thrown, incised, glazes meet at the rim (pour-glazed inside, waxed, dip-glazed outside).
| Glossary |
Metal Oxides
Metal oxide powders are used in ceramics to produce color. But a life time is not enough to study the complexities of their use and potential in glazes, engobes, bodies and enamels. |
| Articles |
Leaching Cone 6 Glaze Case Study
An example of how we can use INSIGHT software to determine of a glaze is likely to leach |
| Materials |
Copper Carbonate
A source of CuO copper oxide used in ceramic glazes to produce a variety of colors (used only or with other colorants). |
| Materials |
Copper Oxide Red
|
| Materials |
Copper Carbonate Basic
This form of copper carbonate is the article of commerce, a mixture of theoretical copper carbonate and copper hydroxide. |
| Hazards |
Copper Oxide and Carbonate
|
| Hazards |
Copper Compounds Toxicology
|
| Typecodes |
Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials. |
| Typecodes |
Colorant
Metallic based materials that impart fired color to glazes and bodies. |
| Oxides | CuO - Cupric Oxide |
| Temperatures | Copper oxide melts (1325-) |
| Temperatures | Copper Oxide breakdown (1025-1325) |
| Frit Softening Point | ~1400C M |
|---|---|
| Density (Specific Gravity) | 6.45 |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk