Copper Hydroxide

Alternate Names: Copper(II) hydroxide, Copper Hydrate, Cupric Hydroxide

Formula: Cu(OH)2

Oxide Analysis Formula Tolerance
CuO 81.53% 1.00
H2O 18.46%n/a
Oxide Weight 79.54
Formula Weight 97.55

Notes

CAS 20427-59-2
This is less reactive than copper carbonate basic and more reactive than cupric oxide (CuO). This material does not contribute to CO2 bubbling in glazes.

Copper Hydroxide has a fairly complex decomposition as it is heated to melting point. Around 185C it loses about 18% weight as it decomposes to the heat stable CuO (cupric oxide) which remains stable until 1000C. Around 1050C about 6.5% is lost, likely involving partial loss of oxygen to form a mix of cuprous and cupric oxides.

Please check the accompanying curve to see the history of weight loss as this is fired (courtesty of Bob Hickerson, World Metal, LLC). You can see how much weight it lost, where it occurs and how fast it happens. Compare this with Copper Carbonate Basic to see the difference.

Related Information


This picture has its own page with more detail, click here to see it.

TGA/DTA curve showing weight loss over temperature range


This picture has its own page with more detail, click here to see it.

Copper Phosphate2


This picture has its own page with more detail, click here to see it.

Copper In Calcite


This picture has its own page with more detail, click here to see it.

Copper

Links

Materials Copper Carbonate
A source of CuO copper oxide used in ceramic glazes to produce a variety of colors (used only or with other colorants).
Materials Mysorine
Materials Copper Carbonate Basic
This form of copper carbonate is the article of commerce, a mixture of theoretical copper carbonate and copper hydroxide.
Typecodes Colorant
Metallic based materials that impart fired color to glazes and bodies.
Hazards Copper Compounds Toxicology
Temperatures Copper hydroxide decomposes to CuO (185-)
URLs http://en.wikipedia.org/wiki/Copper(II)_hydroxide
Copper Hydroxide at Wikipedia

Data

TGA See accompanying chart picture

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy