0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Co-efficient of Thermal Expansion | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Substitution | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silica:Alumina Ratio | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Opacifier

Glaze opacity refers to the degree to which it is opaque. Opacifiers are powders added to transparent ceramic glazes to make them opaque.

Key phrases linking here: opacification, opacifiers, opacifier, opacify - Learn more

Details

A glaze additive that impart opacity, transforming an otherwise transparent glaze into an opaque one. Common opacifiers are tin oxide and zircon compounds. Opacifiers typically work by simply not dissolving into the melt, the white suspended particles thus reflect and scatter the light. Since they do not participate in the chemistry of the melt, they are typically rationalized at the recipe level (their effect on thermal expansion, development of colors and glaze hardness are obvious factors).

Another mechanism of opacity is crystallization, which can occur when a crystallizing ingredient is supersaturated into the mix (e.g. TiO2) or when slow cooling a glaze to encourage crystallization of less saturated oxides that crystallize easily (e.g. boron blue). This mechanism is more likely to produce a glass that cutlery marks.

A third mechanism is suspended micro-bubbles that cloud the glass. These are often candidates for being able to use lower opacifer percentages.

Opacified glazes can be more subject to cutlery marking. This is especially the case when a glaze is simply not melting to as smooth a surface. The addition of refractory zircon opacifier is a case in point: Jagged edges of microscopic particles can protrude out of the surface.

When opacifiers are added to pigmented glazes, color depth and intensity are lost. However, consistency of color is gained because changes in thickness are less prone to changes in tone or intensity. A disadvantage of pacifying color glazes is that higher percentages of stain are needed to get intense color.

Related Information

G1214Z1 at cone 6 with 10% Zircopax and 5% tin oxide


This picture has its own page with more detail, click here to see it.

The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. The tin is on the right.

5% titanium dioxide in G2934Y matte, G1214Z1 matte, G2926B glossy


This picture has its own page with more detail, click here to see it.

The body is Plainsman M390. The firing schedule is Plainsman PLC6DS. Of course, rutile could be used in place of titanium; it contains iron oxide that would enhance the development of blue. A small amount of cobalt can also be added to enhance the blue (the G2934 magnesia matte on the left, especially, will respond to that).

G2934 Cone 6 Matte with 10% Zircopax and 5% tin oxide


This picture has its own page with more detail, click here to see it.

The body is Plainsman M390. The firing schedule is Plainsman PLC6DS.

G2926B cone 6 transparent with 10% Zircopax and 5% tin oxide


This picture has its own page with more detail, click here to see it.

The body is Plainsman M390. The firing schedule is Plainsman PLC6DS.

How do you turn a transparent glaze into a white?


This picture has its own page with more detail, click here to see it.

Right: Ravenscrag GR6-A transparent base glaze. Left: It has been opacified (turned opaque) by adding 10% Zircopax. This opacification mechanism can be transplanted into almost any transparent glaze. It can also be employed in colored transparents, it will convert their coloration to a pastel shade, lightening it. Zircon works well in oxidation and reduction. Tin oxide is another opacifier, it is much more expensive and only works in oxidation firing.

Zircon glazes cover well but they have a problem


This picture has its own page with more detail, click here to see it.

This sanitary ware tank lid was made in China. Notice how thick the white glaze is being applied to cover the iron containing body below. This is a testament to how opaque a zircon opacified glaze can be. Zircon often causes crawling (likely due to a combination of the effects of its fine particle size on drying properties and its tendency to stiffen the melt). Extra measures and constant attention to detail (e.g. glaze thickness, slurry rheology, avoidance of sharp contours on ware) are needed with such glazes.

Titanium as an opacifier


This picture has its own page with more detail, click here to see it.

This is a lithium glaze fired at cone 6. It has 6% titanium. This effect will also work in other types of transparent recipes. There should be more blue with slower cooling. Mixing some rutile in (e.g. 4 titanium, 2 rutile) should enhance also. 6% is pushing the edge of how much titanium should be in a recipe. Any more, or cooling too slow, could transform the surface into a mass of white crystals (which would be rough and non-functional). It is best to manually program firings, the up and down schedules? That would make the result consistent no matter how heavily or lightly loaded a kiln is.

Don't waste expensive tin oxide, propeller mix glazes well


Tin oxide in glaze needs thorough mixing

This picture has its own page with more detail, click here to see it.

This is a cone 04 glaze on a terra cotta body. Two 300-gram test batches were made. Both have 5% tin oxide added to a base transparent, G1916Q. The one on the left was high-speed propeller-mixed for 10 seconds. That was not enough, small agglomerates appear as tiny white specks floating in the glass. The one on the right was blender mixed for 60 seconds. Now the incredibly small tin particles have been dispersed and can do their job of opacifying the glaze. Would sieving the slurry have worked? No, the particle agglomerates can be far smaller than the openings in an 80-mesh sieve (individual particles could be 1000 times smaller!). The thorough dispersion of the expensive tin oxide particles has real benefit: It enables making an accurate assessment of whether the 5% addition is enough. In this case it isn't, more is needed.

White spots and blisters in a high zircon glaze at cone 6


This picture has its own page with more detail, click here to see it.

This is also a common problem at low fire on earthenware clay (but can also appear on a buff stonewares). Those white spots you see on the beetle also cover the entire glaze surface (although not visible). They are sites of gas escaping (from particles decomposing in the body). The spots likely percolate during soaking at top temperate. Some of them, notably on the almost vertical inner walls of this bowl, having not smoothed over during cool down.

What can you do? Use the highest possible bisque temperature, even cone 02 (make the glaze thixotropic so it will hang on to the denser body, see the link below about this). Adjust the glaze chemistry to melt later after gassing has finished (more zinc, less boron). Apply a thinner glaze layer (more thixotropy and lower specific gravity will enable a more even coverage with less thickness). Instead of soaking at temperature, drop 100 degrees and soak there instead (gassing is much less and the increasing viscosity of the melt overcomes the surface tension). Use a body not having any large particles that decompose (and gas) on firing. Use cones to verify the temperature your electronic controller reports.

DIY the commercial glaze on mug #1:

You must consider five factors to make it work


This picture has its own page with more detail, click here to see it.

The mug on the left, #1, is a commercial brushing glaze. It is opaque enough to cover this red-burning clay body. It shows the desired effect. That depends on the fact that opaque glazes stretch thinner on the sharp edges of incised designs. If they have enough melt mobility and are applied right, the effect is amplified. This potter is attempting to mix her own DIY equivalent as a dipping glaze, adding 4% tin oxide to a transparent base glaze in #2 and zircon (a higher percentage) in #3. As you can see, the effect is not working as well, and there are several reasons:

#2 is whiter because it uses tin oxide as the opacifier (vs. zircon, likely used in #1). #2 and #3 have less melt fluidity; the base is likely G2926B. #1 was applied by brush, the others using a dipping glaze. Matching the original involves a combination of things: A base having more flux (especially B2O3) is needed (e.g. G3806C). Careful control of application thickness. The right percentage of opacifier. And, it may be necessary to mix the DIY version as a brushing glaze, that method of application might be needed to get the careful control of thickness and thickness variation needed.

In pigmented glossy transparent glazes

The pigment is the opacifier


This picture has its own page with more detail, click here to see it.

This is a cone 6 oxidation transparent glaze having enough flux (from a boron frit) to make it melt very well, that is why it is running and pooling. Iron oxide has been added (around 5%), producing this transparent amber effect. Darker coloration occurs where the glaze has run thicker (because it absorbs more light). This simple mechanism enables the glaze to automatically highlight contours, emboss and textures on the underlying surface. This mechanism works with any color in almost any transparent base glaze, as long as bubble clouding and crystallization do not occur. Entire lines of commercial glazes (e.g. AMACO Celadons) are based on this mechanism and potters prize it (industry doesn't like it because it is difficult to achieve consistency).

This glaze relies on high levels of K2O and Na2O to produce the brilliant gloss, however the side effect of that is crazing. These are sourced by feldspars, nepheline syenite and are high in certain frits. To achieve this effect, recipes must rely on other fluxes like boron, lithium or zinc.

Our base glazes plus opacifiers on a dark burning body at cone 6


Red burning clay tiles with opacified versions of G2926B, G2934, G1214Z

This picture has its own page with more detail, click here to see it.

The body is Plainsman M390. These are commonly used base glazes. The top one is a magnesia matte, next down is a calcia matte. They react very differently to these additions. Notice also the difference when titanium dioxide is applied thickly. Tin oxide fires whiter than zircon (e.g. Zircopax). Each opacifier has issues. Tin is expensive. Titanium is difficult to mix into the slurry (screening required), not as white or opaque, variations in thickness produce more difference in results and it can turn blue. Zircon is more likely to cutlery mark, twice as much is required and it amplifies the color of any iron present.

Two cone 6 matte glazes opacified with 10% Zircopax


This picture has its own page with more detail, click here to see it.

The clay is a buff stoneware. The upper two samples are G2934, a magnesia matte. The one on the right has 10% zircon added to opacify. The bottom two are G1214Z1 (transparent version and opacified-with-zircon version). The difference is surface character is visible.

The best way to opacify a low-temperature terra cotta glaze


Opacify a low fire transparent glaze

This picture has its own page with more detail, click here to see it.

Tin oxide is a powerful opacifier, but the 5% in this Frit 3124 based Arbuckle Majolica cone 04 recipe on the left is not sufficient. Adding 10% zircon (e.g. Zircopax, Superpax) produces the one on the right. Would just using 15% zircon be better? No. More zircon means a stiffer melt and more issues with crawling (notice the small bare spots on the right edge). This could be managed by the addition of CMC gum or a higher clay content to get better adhesion and dry hardness). But another improvement would be worth trying first: Use 4% tin and 8% zircon. That should opacify enough and present fewer problems with crawling.

White stain. Does it work?


This picture has its own page with more detail, click here to see it.

This is G2934Y matte glaze base with opacifiers added. It has been applied to a dark-burning body to demonstrate the comparative degrees of opacity. The stain is Mason 6700 white. While it does not opacify nearly as well as tin or zircon, it does produce a smoother surface.

A hazard of using titanium opacifier in a glaze


A titanium opacified glaze on a mug

This picture has its own page with more detail, click here to see it.

On a clay test tile this titanium opacified cone 6 oxidation glaze, G1214Z1, looks great. But it is important to recognize that its variegated fired appearance is a combination multiple factors: The chemistry of the glaze, the titanium, quality laydown, the PLC6DS firing schedule, the red M390 clay body and variations in the thickness-of-application. However, the last four of those factors changed with the mug on the right! It is made from buff-burning M340! There are drips from uneven drainage during glazing. The slow cool C6DHSC firing schedule. Notice how it is actually going transparent where very thick. An even laydown was not achieved since the slurry was not properly mixed, it contains calcined kaolin and requires special attention to achieve a thixotropy.

Toilet bowl glaze vs. variegated glaze


This picture has its own page with more detail, click here to see it.

Most artists and potters want some sort of visual variegation in their glazes. The cone 6 oxidation mug on the right demonstrates several types. Opacity variation with thickness: The outer blue varies (breaks) to brown on the edges of contours where the glaze layer is thinner. Phase changes: The rutile blue color swirls within because of phase changes within the glass (zones of differing chemistry). Crystallization: The inside glaze is normally a clear amber transparent, but because these were slow cooling in the firing, iron in the glass has crystallized on the surface. Clay color: The mugs are made from a brown clay, the iron within it is bleeding into the blue and amplifying color change on thin sections.

Two stains. 4 colors. Will the guilty oxide please step forward.


One stain produces clear in one glaze and red in another. Another stain blue and purple. Why?

This picture has its own page with more detail, click here to see it.

These pairs are G2934 matte and G2916F glossy cone 6 base glaze recipes. The left pair has 5% maroon stain added, the right pair 5% purple stain. Why? The Mason Colorworks reference guide has the same precaution for both stains: the host glaze must be zincless and have 6.7-8.4% CaO (this is a little unclear, it is actually expressing a minimum, the more the CaO the better). The matte recipe calculates to 11% CaO, the glossy to 9%. So there is enough CaO. The problem is MgO (it is the mechanism of the matteness in the left two), it impedes the development of both colors (although not mentioned on the Mason docs).

Adding Zircopax to G2571A dolomite matte


This picture has its own page with more detail, click here to see it.

On the left: G2571A dolomite matte fired at cone 10R. Right: 10% Zircopax has been added. Both are on a buff stoneware (H550 from Plainsman Clays).

Does Zircopax only whiten and opacify a clear glaze? No.


This picture has its own page with more detail, click here to see it.

This GLFL test for melt flow demonstrates how zircon opacifies but also stiffens a glaze melt at cone 6. Zircon also hardens many glazes, even if used in smaller amounts than will opacify.

5% tin oxide in a transparent boron cone 6 glaze


This picture has its own page with more detail, click here to see it.

This is a 45:27:28 Gerstley Borate:Kaolin:Silica base on a dark firing clay body. But tin oxide will do that in almost any cone 6 clear glaze (use one that fits your clay body).

Why is this transparent so full of bubbles?


This picture has its own page with more detail, click here to see it.

An example of how a micro-bubble population in the matrix of a transparent glaze can partially opacify it. If this glaze was completely transparent, the red clay body would show much better. However this is not the fault of the glaze. On a white body it would be more transparent. The problem is the terra cotta body. This is fired at cone 02. As the body approaches vitrification the decomposition of particles within it generate gases that bubble up in to the glaze. A positive aspect of this phenomena that this glaze could be opacified using a lower percentage of zircon.

This type of glaze responds better to opacifier additions.

What happens when you opacify a colored glaze?


This picture has its own page with more detail, click here to see it.

Left: G2934 cone 6 matte glaze with 3% Mason 6300 blue stain. Right: An additional 4% tin added. The thickness of application is close to the same. Notice how an opacified color does not have depth and therefore is lighter in color. Also it does not break to different shades at the edges of contours the way the transparent color does.

A good matte glaze. A bad matte glaze.


This picture has its own page with more detail, click here to see it.

A melt fluidity comparison between two cone 6 matte glazes. G2934 is an MgO saturated boron fluxed glaze that melts to the right degree, forms a good glass, has a low thermal expansion, resists leaching and does not cutlery mark. G2000 is a much-trafficked cone 6 recipe, it is fluxed by zinc to produce a surface mesh of micro-crystals that not only mattes but also opacifies the glaze. But it forms a poor glass, runs too much, cutlery marks badly, stains easily, crazes and is likely not food safe! The G2934 recipe is google-searchable and a good demonstration of how the high-MgO matte mechanism (from talc) creates a silky surface at cone 6 oxidation the same as it does at cone 10 reduction (from dolomite). However it does need a tin or zircon addition to be white.

Adding an opacifier can produce cutlery marking


Opacified glaze is cutlery marking

This picture has its own page with more detail, click here to see it.

This is G2934 cone 6 matte (left) with 10% zircon (center), 4% tin oxide (right). Although the base unopacified recipe does not cutlery mark the other two do. Although the marks clean off all of the two on the right, the zircon version (in this case Zircopax) version has the worst and is difficult to clean. Thus, a small change is all that is likely needed. One solution is to reduce the matteness of this glaze, moving to more toward a satin surface. A way to do this is to line-blend in a glossy glaze to create a compromise between the most matteness possible yet a surface that does not mark or stain. Another option is to switch to 400 mesh silica in the recipe, that will enable many more of the particles to go into solution in the melt, thus increasing the gloss a little (an improving the firing surface in other ways).

The action of Zircopax vs Tin Oxide at cone 10R


This picture has its own page with more detail, click here to see it.

On Plainsman H443 iron stoneware in reduction firing. Notice Tin does not work. Also notice that between 7.5 and 10% Zircopax provides as much opacity as does 15% (Zircon is very expensive).

Inbound Photo Links


A grid of fired glaze test samples showing opacifiers perform in four glazes
Zircopax, tin oxide, titanium as opacifiers in four base glazes

Links

Glossary Base Glaze
Understand your a glaze and learn how to adjust and improve it. Build others from that. We have bases for low, medium and high fire.
Glossary Variegation
Ceramic glaze variegation refers to its visual character. This is an overview of the various mechanisms to make glazes dance with color, crystals, highlights, speckles, rivulets, etc.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Colorant
In ceramics and pottery, colorants are added to glazes as metal oxides, metal-oxide-containing raw materials or as manufactured stains.
Glossary Boron Blue
Boron blue is a glaze fault involving the crystallization of calcium borate. It can be solved using glaze chemistry.
Glossary Cutlery Marking
Ceramic glazes that mark from cutlery are either not properly melted (lack flux), melted too much (lacking SiO2 and Al2O3), or have a micro-abrasive surface that abrades metal from cutlery.
Glossary Majolica
Majolica is a tradition of Italian Renaissance white opaque glazed red earthenware having brightly colored brushwork decoration. Knowing some technical details will help you better succeed with the process.
Glossary Opacity
Opacity of ceramics glazes is normally achieved by adding an opacifier like tin oxide or zircon. However, there are chemical profiles that can turn transparent glazes milky and make it cheaper to opacify them.
Properties Glaze Opacifier
Properties Glaze Variegation
Projects Properties
Materials Titanium Dioxide
A super white powder used in ceramic glazes to variegate, opacify and moderate color.
Materials Tin Oxide
Its principle use in ceramics is as an opacifier in glazes. It is very expensive.
Typecodes Opacifier
Opacifiers are powders that turn transparent glazes opaque by various chemical and physical mechanisms (and combinations of mechanisms).

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy