3898 | 3897 | 3896 | 3895 | 3890 | 3891 | 3892 | 3887 | 3888 | 3889 | 3883 | 3885 | 3882 | 3880 | 3881 | 3878 | 3877 | 3876 | 3871 | 3872 | 3874 | 3869 | 3870 | 3866 | 3867 | 3864 | 3863 | 3862 | 3861 | 3860 | 3859 | 3838 | 3857 | 3858 | 3855 | 3856 | 3851 | 3853 | 3854 | 3849 | 3850 | 3852 | 3846 | 3848 | 3843 | 3840 | 3841 | 3842 | 3837 | 3836 | 3833 | 3831 | 3832 | 3829 | 3827 | 3828 | 3826 | 3824 | 3823 | 3822 | 3820 | 3819 | 3818 | 3815 | 3816 | 3817 | 3814 | 3813 | 3811 | 3810 | 3806 | 3807 | 3808 | 3805 | 3803 | 3802 | 3801 | 3800 | 3797 | 3798 | 3796 | 3793 | 3794 | 3792 | 3789 | 3786 | 3784 | 3787 | 3781 | 3779 | 3775 | 3773 | 3774 | 3772 | 3767 | 3768 | 3769 | 3762 | 3760 | 3759 | 3755 | 3752 | 3753 | 3754 | 3750 | 3748 | 3749 | 3742 | 3743 | 3745 | 3746 | 3747 | 3740 | 3737 | 3738 | 3739 | 3736 | 3734 | 3733 | 3732 | 3731 | 3729 | 3728 | 3726 | 3725 | 3724 | 3723 | 3721 | 3719 | 3720 | 3718 | 3716 | 3713 | 3712 | 3711 | 3710 | 3709 | 3707 | 3708 | 3706 | 3705 | 3704 | 3702 | 3701 | 3700 | 3699 | 3698 | 3695 | 3696 | 3697 | 3692 | 3693 | 3694 | 3690 | 3691 | 3689 | 3688 | 3685 | 3686 | 3679 | 3678 | 3676 | 3675 | 3674 | 3672 | 3673 | 3663 | 3664 | 3661 | 3656 | 3657 | 3658 | 3659 | 3651 | 3652 | 3654 | 3655 | 3650 | 3649 | 3648 | 3646 | 3647 | 3644 | 3645 | 3643 | 3642 | 3640 | 3639 | 3637 | 3636 | 3634 | 3635 | 3632 | 3631 | 3629 | 3630 | 3626 | 3627 | 3624 | 3625 | 3622 | 3623 | 3620 | 3619 | 3612 | 3610 | 3611 | 3606 | 3607 | 3608 | 3609 | 3602 | 3603 | 3604 | 3605 | 3601 | 3600 | 3599 | 3598 | 3596 | 3595 | 3594 | 3593 | 3591 | 3592 | 3588 | 3589 | 3585 | 3586 | 3584 | 3580 | 3581 | 3582 | 3583 | 3579 | 3577 | 3578 | 3576 | 3574 | 3572 | 3573 | 3571 | 3570 | 3568 | 3567 | 3565 | 3562 | 3563 | 3560 | 3561 | 3559 | 3557 | 3556 | 3555 | 3554 | 3553 | 3551 | 3552 | 3550 | 3549 | 3548 | 3547 | 3546 | 3544 | 3545 | 3543 | 3542 | 3538 | 3539 | 3540 | 3541 | 3536 | 3537 | 3535 | 3534 | 3531 | 3532 | 3533 | 3529 | 3530 | 3527 | 3528 | 3526 | 3525 | 3524 | 3523 | 3522 | 3520 | 3518 | 3516 | 3517 | 3515 | 3514 | 3512 | 3513 | 3511 | 3510 | 3509 | 3508 | 3507 | 3506 | 3505 | 3504 | 3046 | 3503 | 3493 | 3494 | 3490 | 3491 | 3486 | 3489 | 3485 | 3481 | 3483 | 3492 | 3479 | 3480 | 3476 | 3477 | 3474 | 3473 | 3471 | 3470 | 3469 | 3468 | 3465 | 3466 | 3467 | 3463 | 3459 | 3460 | 3461 | 3462 | 3458 | 3457 | 3456 | 3455 | 3454 | 3452 | 3449 | 3448 | 3447 | 3446 | 3445 | 3443 | 3444 | 3442 | 3441 | 3439 | 3440 | 3437 | 3438 | 3435 | 3436 | 3431 | 3433 | 3434 | 3430 | 3427 | 3428 | 3425 | 3426 | 3423 | 3422 | 3419 | 3421 | 3418 | 3415 | 3416 | 3417 | 3414 | 3413 | 3411 | 3412 | 3409 | 3410 | 3408 | 3401 | 3402 | 3403 | 3404 | 3406 | 3407 | 3400 | 3399 | 3397 | 3393 | 3394 | 3396 | 3392 | 3391 | 3387 | 3389 | 3390 | 3385 | 3384 | 3383 | 3382 | 3379 | 3380 | 3381 | 3378 | 3376 | 3375 | 3374 | 3373 | 3372 | 3370 | 3367 | 3368 | 3369 | 3364 | 3363 | 3360 | 3359 | 3358 | 3356 | 3355 | 3354 | 3352 | 3349 | 3348 | 3347 | 3344 | 3345 | 3346 | 3343 | 3342 | 3340 | 3338 | 3339 | 3337 | 3335 | 3336 | 3334 | 3333 | 3330 | 3322 | 3319 | 3320 | 3321 | 3317 | 3316 | 3313 | 3314 | 3315 | 3312 | 3310 | 3311 | 3309 | 3307 | 3308 | 3306 | 3304 | 3303 | 3302 | 3300 | 3301 | 3298 | 3299 | 3296 | 3295 | 3293 | 3294 | 3292 | 3291 | 3290 | 3289 | 3288 | 3286 | 3285 | 3284 | 3280 | 3281 | 3282 | 3278 | 3277 | 3272 | 3273 | 3274 | 3275 | 3276 | 3271 | 3270 | 3267 | 3268 | 3265 | 3266 | 3264 | 3262 | 3261 | 3260 | 3259 | 3258 | 3257 | 3256 | 3255 | 3253 | 3254 | 3251 | 3248 | 3247 | 3245 | 3246 | 3244 | 3241 | 3239 | 3236 | 3237 | 3235 | 3234 | 3233 | 3231 | 3232 | 3230 | 3229 | 3201 | 3202 | 3203 | 3204 | 3205 | 3206 | 3207 | 3208 | 3209 | 3210 | 3211 | 3212 | 3213 | 3214 | 3215 | 3216 | 3217 | 3219 | 3220 | 3222 | 3223 | 3224 | 3226 | 3227 | 3228 | 3199 | 3198 | 3197 | 3195 | 3196 | 3191 | 3192 | 3193 | 3194 | 3188 | 3189 | 3187 | 3185 | 3186 | 3183 | 3181 | 3182 | 3179 | 3180 | 3177 | 3176 | 3175 | 3174 | 3173 | 3169 | 3167 | 3164 | 3162 | 3159 | 3158 | 3157 | 3154 | 3155 | 3156 | 3153 | 3149 | 3150 | 3144 | 3145 | 3146 | 3147 | 3148 | 3142 | 3143 | 3139 | 3141 | 3138 | 3136 | 3137 | 3132 | 3135 | 3131 | 3130 | 3127 | 3124 | 3125 | 3126 | 3122 | 3123 | 3121 | 3120 | 3117 | 3119 | 3116 | 3112 | 3113 | 3114 | 3109 | 3110 | 3111 | 3098 | 3099 | 3102 | 3103 | 3104 | 3105 | 3106 | 3107 | 3108 | 3096 | 3094 | 3095 | 3091 | 3092 | 3093 | 3089 | 3090 | 3087 | 3086 | 3082 | 3083 | 3084 | 3080 | 3081 | 3079 | 3078 | 3077 | 3074 | 3075 | 3076 | 3073 | 3072 | 3070 | 3053 | 3055 | 3056 | 3057 | 3058 | 3059 | 3060 | 3061 | 3062 | 3063 | 3064 | 3065 | 3066 | 3067 | 3068 | 3069 | 3052 | 3050 | 3051 | 3048 | 3049 | 3047 | 3044 | 3043 | 3042 | 3041 | 3040 | 3038 | 3039 | 3037 | 3036 | 3035 | 3034 | 3033 | 3029 | 3030 | 3031 | 3023 | 3024 | 3021 | 3022 | 3019 | 3016 | 3017 | 3018 | 3015 | 3012 | 3013 | 3014 | 3011 | 3010 | 3007 | 3008 | 3009 | 3005 | 3006 | 3004 | 3001 | 3002 | 3003 | 2999 | 2995 | 2996 | 2994 | 2991 | 2992 | 2993 | 2990 | 2989 | 2986 | 2987 | 2988 | 2982 | 2983 | 2984 | 2985 | 2979 | 2980 | 2976 | 2977 | 2974 | 2973 | 2970 | 2971 | 2967 | 2968 | 2969 | 2966 | 2964 | 2965 | 2963 | 2961 | 2962 | 2960 | 2958 | 2952 | 2953 | 2954 | 2955 | 2956 | 2950 | 2951 | 2948 | 2949 | 2945 | 2946 | 2947 | 2944 | 2943 | 2939 | 2940 | 2941 | 2942 | 2937 | 2938 | 2936 | 2935 | 2929 | 2930 | 2931 | 2932 | 2933 | 2934 | 2928 | 2927 | 2925 | 2926 | 2921 | 2922 | 2923 | 2924 | 2919 | 2920 | 2917 | 2918 | 2915 | 2916 | 2913 | 2914 | 2912 | 2911 | 2910 | 2909 | 2907 | 2908 | 2906 | 2905 | 2903 | 2904 | 2900 | 2899 | 2898 | 2893 | 2894 | 2895 | 2896 | 2897 | 2890 | 2891 | 2892 | 2887 | 2888 | 2889 | 2885 | 2882 | 2883 | 2884 | 2880 | 2881 | 2878 | 2877 | 2872 | 2873 | 2874 | 2875 | 2876 | 2871 | 2868 | 2869 | 2870 | 2866 | 2867 | 2865 | 2864 | 2862 | 2863 | 2861 | 2860 | 2858 | 2859 | 2856 | 2857 | 2854 | 2855 | 2853 | 2852 | 2848 | 2849 | 2850 | 2847 | 2845 | 2846 | 2843 | 2842 | 2840 | 2841 | 2839 | 2838 | 2837 | 2836 | 2835 | 2833 | 2834 | 2832 | 2831 | 2828 | 2829 | 2827 | 2826 | 2825 | 2824 | 2822 | 2823 | 2820 | 2821 | 2819 | 2816 | 2815 | 2814 | 2813 | 2812 | 2811 | 2793 | 2794 | 2795 | 2796 | 2797 | 2798 | 2799 | 2800 | 2801 | 2802 | 2803 | 2804 | 2805 | 2806 | 2807 | 2808 | 2809 | 2810 | 2791 | 2792 | 2790 | 2787 | 2788 | 2784 | 2785 | 2786 | 2781 | 2782 | 2780 | 2777 | 2778 | 2779 | 2776 | 2775 | 2774 | 2772 | 2771 | 2769 | 2770 | 2768 | 2767 | 2766 | 2764 | 2765 | 2762 | 2763 | 2761 | 2760 | 2759 | 2758 | 2756 | 2752 | 2753 | 2754 | 2755 | 2750 | 2751 | 2748 | 2749 | 2747 | 2745 | 2746 | 2742 | 2743 | 2740 | 2741 | 2739 | 2737 | 2738 | 2736 | 2735 | 2734 | 2733 | 2732 | 2729 | 2730 | 2731 | 2728 | 2727 | 2726 | 2723 | 2724 | 2725 | 2722 | 2719 | 2720 | 2721 | 2718 | 2716 | 2715 | 2714 | 2713 | 2712 | 2711 | 2709 | 2708 | 2706 | 2707 | 2704 | 2705 | 2703 | 2702 | 2700 | 2693 | 2694 | 2695 | 2696 | 2697 | 2698 | 2699 | 2692 | 2690 | 2691 | 2689 | 2688 | 2687 | 2686 | 2685 | 2684 | 2683 | 2680 | 2681 | 2682 | 2678 | 2679 | 2677 | 2676 | 2675 | 2674 | 2673 | 2672 | 2671 | 2670 | 2669 | 2666 | 2668 | 2664 | 2665 | 2662 | 2663 | 2660 | 2661 | 2656 | 2657 | 2658 | 2659 | 2655 | 2654 | 2653 | 2652 | 2649 | 2650 | 2651 | 2646 | 2647 | 2648 | 2643 | 2644 | 2641 | 2642 | 2639 | 2640 | 2637 | 2638 | 2635 | 2636 | 2633 | 2634 | 2631 | 2632 | 2630 | 2629 | 2627 | 2628 | 2624 | 2626 | 2621 | 2622 | 2623 | 2618 | 2619 | 2617 | 2614 | 2615 | 2616 | 2613 | 2612 | 2607 | 2608 | 2609 | 2611 | 2606 | 2605 | 2602 | 2603 | 2604 | 2600 | 2601 | 2599 | 2598 | 2597 | 2595 | 2596 | 2591 | 2592 | 2593 | 2594 | 2585 | 2586 | 2587 | 2588 | 2589 | | 2584 | 2583 | 2582 | 2581 | 2578 | 2580 | 2576 | 2577 | 2573 | 2574 | 2575 | 2572 | 2571 | 2566 | 2567 | 2569 | 2570 | 2563 | 2565 | 2562 | 2561 | 2560 | 2558 | 2559 | 2557 | 2556 | 2554 | 2555 | 2551 | 2552 | 2548 | 2549 | 2550 | 2547 | 2545 | 2546 | 2542 | 2543 | 2544 | 2540 | 2541 | 2539 | 2537 | 2536 | 2533 | 2534 | 2535 | 2531 | 2532 | 2530 | 2528 | 2525 | 2526 | 2527 | 2522 | 2523 | 2521 | 2519 | 2520 | 2518 | 2517 | 2516 | 2515 | 2514 | 2513 | 2511 | 2512 | 2509 | 2510 | 2508 | 2506 | 2507 | 2505 | 2504 | 2503 | 2502 | 2501 | 2499 | 2490 | 2494 | 2495 | 2496 | 2497 | 2498 | 2489 | 2488 | 2487 | 2486 | 2485 | 2484 | 2483 | 2482 | 2481 | 2479 | 2480 | 2478 | 2474 | 2475 | 2476 | 2477 | 2472 | 2473 | 2471 | 2470 | 2465 | 2466 | 2467 | 2468 | 2469 | 2464 | 2461 | 2460 | 2459 | 2458 | 2457 | 2454 | 2455 | 2456 | 2451 | 2452 | 2453 | 2449 | 2450 | 2447 | 2448 | 2442 | 2443 | 2444 | 2445 | 2446 | 2440 | 2441 | 2439 | 2436 | 2437 | 2438 | 2434 | 2435 | 2433 | 2432 | 2429 | 2430 | 2431 | 2425 | 2426 | 2427 | 2428 | 2422 | 2423 | 2424 | 2421 | 2417 | 2418 | 2419 | 2420 | 2416 | 2415 | 2412 | 2411 | 2410 | 2408 | 2409 | 2407 | 2406 | 2405 | 2403 | 2404 | 2402 | 2401 | 2400 | 2399 | 2398 | 2397 | 2396 | 2395 | 2394 | 2392 | 2393 | 2390 | 2389 | 2387 | 2386 | 2385 | 2384 | 2383 | 2380 | 2375 | 2376 | 2377 | 2378 | 2379 | 2374 | 2373 | 2372 | 2371 | 2369 | 2370 | 2366 | 2368 | 2361 | 2362 | 2363 | 2364 | 2365 | 2360 | 2359 | 2355 | 2356 | 2357 | 2354 | 2353 | 2350 | 2351 | 2348 | 2349 | 2346 | 2347 | 2344 | 2345 | 2343 | 2342 | 2341 | 2337 | 2339 | 2340 | 2335 | 2336 | 2334 | 2333 | 2328 | 2329 | 2330 | 2331 | 2332 | 2327 | 2326 | 2323 | 2324 | 2325 | 2322 | 2321 | 2316 | 2317 | 2318 | 2319 | 2320 | 2314 | 2315 | 2311 | 2312 | 2313 | 2309 | 2308 | 2306 | 2307 | 2304 | 2305 | 2303 | 2299 | 2300 | 2301 | 2297 | 2294 | 2295 | 2296 | 2292 | 2278 | 2279 | 2280 | 2282 | 2283 | 2284 | 2285 | 2286 | 2287 | 2288 | 2289 | 2290 | 2273 | 2274 | 2275 | 2276 | 2277 | 2271 | 2270 | 2269 | 2266 | 2265 | 2263 | 2264 | 2262 | 2260 | 2261 | 2259 | 2258 | 2257 | 2255 | 2256 | 2254 | 2250 | 2252 | 2249 | 2247 | 2248 | 2246 | 2242 | 2243 | 2245 | 2239 | 2240 | 2241 | 2235 | 2236 | 2237 | 2238 | 2234 | 2233 | 2232 | 2231 | 2230 | 2229 | 2225 | 2226 | 2224 | 2222 | 2223 | 2220 | 2221 | 2218 | 2219 | 2216 | 2217 | 2214 | 2215 | 2213 | 2211 | 2212 | 2210 | 2209 | 2208 | 2207 | 2206 | 2205 | 2203 | 2204 | 2202 | 2201 | 2199 | 2200 | 2198 | 2197 | 2195 | 2196 | 2194 | 2192 | 2193 | 2191 | 2189 | 2190 | 2188 | 2186 | 2187 | 2185 | 2184 | 2182 | 2183 | 2180 | 2178 | 2179 | 2176 | 2177 | 2172 | 2173 | 2174 | 2175 | 2171 | 2166 | 2167 | 2169 | 2170 | 2165 | 2156 | 2157 | 2158 | 2159 | 2161 | 2162 | 2164 | 2153 | 2154 | 2155 | 2151 | 2150 | 2148 | 2149 | 2142 | 2143 | 2144 | 2145 | 2146 | 2147 | 2140 | 2141 | 2138 | 2139 | 2136 | 2137 | 2135 | 2129 | 2130 | 2131 | 2132 | 2133 | 2134 | 2128 | 2127 | 2126 | 2125 | 2124 | 2121 | 2122 | 2123 | 2118 | 2117 | 2115 | 2116 | 2114 | 2113 | 2112 | 2111 | 2109 | 2108 | 2107 | 2106 | 2104 | 2105 | 2101 | 2102 | 2103 | 2099 | 2100 | 2096 | 2094 | 2095 | 2093 | 2092 | 2091 | 2089 | 2090 | 2088 | 2087 | 2086 | 2085 | 2084 | 2082 | 2083 | 2081 | 2078 | 2079 | 2080 | 2076 | 2077 | 2073 | 2074 | 2075 | 2071 | 2069 | 2066 | 2067 | 2068 | 2064 | 2060 | 2061 | 2062 | 2059 | 2057 | 2058 | 2052 | 2053 | 2054 | 2055 | 2056 | 2049 | 2050 | 2051 | 2048 | 2047 | 2046 | 2042 | 2043 | 2044 | 2045 | 2040 | 2039 | 2038 | 2036 | 2035 | 2029 | 2030 | 2031 | 2033 | 2034 | 2027 | 2024 | 2025 | 2026 | 2017 | 2018 | 2019 | 2020 | 2021 | 2022 | 2016 | 2015 | 2014 | 2013 | 2010 | 2011 | 2012 | 2008 | 2009 | 2007 | 2001 | 2002 | 2003 | 2004 | 2005 | 1993 | 1995 | 1998 | 2000 | 1990 | 1991 | 1987 | 1988 | 1986 | 1983 | 1984 | 1976 | 1977 | 1978 | 1979 | 1980 | 1981 | 1974 | 1975 | 1973 | 1972 | 1970 | 1968 | 1969 | 1967 | 1966 | 1965 | 1964 | 1962 | 1961 | 1959 | 1960 | 1955 | 1956 | 1957 | 1954 | 1952 | 1953 | 1950 | 1951 | 1948 | 1947 | 1946 | 1944 | 1945 | 1940 | 1941 | 1942 | 1943 | 1939 | 1934 | 1935 | 1936 | 1937 | 1938 | 1932 | 1933 | 1931 | 1930 | 1928 | 1927 | 1922 | 1923 | 1924 | 1925 | 1926 | 1916 | 1918 | 1919 | 1920 | 1921 | 1915 | 1914 | 1906 | 1907 | 1908 | 1909 | 1910 | 1911 | 1912 | 1913 | 1902 | 1904 | 1905 | 1895 | 1896 | 1897 | 1899 | 1900 | 1901 | 1891 | 1893 | 1894 | 1890 | 1888 | 1889 | 1887 | 1885 | 1882 | 1883 | 1884 | 1874 | 1875 | 1876 | 1877 | 1878 | 1879 | 1870 | 1871 | 1872 | 1873 | 1868 | 1867 | 1866 | 1865 | 1864 | 1858 | 1859 | 1860 | 1861 | 1862 | 1863 | 1854 | 1855 | 1850 | 1851 | 1852 | 1848 | 1849 | 1846 | 1847 | 1843 | 1844 | 1845 | 1842 | 1831 | 1832 | 1833 | 1834 | 1835 | 1836 | 1838 | 1839 | 1840 | 1841 | 1828 | 1829 | 1830 | 1827 | 1826 | 1825 | 1823 | 1824 | 1818 | 1819 | 1820 | 1821 | 1822 | 1817 | 1815 | 1816 | 1814 | 1812 | 1811 | 1809 | 1810 | 1807 | 1806 | 1805 | 1804 | 1803 | 1802 | 1796 | 1797 | 1798 | 1799 | 1800 | 1801 | 1792 | 1793 | 1794 | 1791 | 1790 | 1789 | 1788 | 1786 | 1785 | 1781 | 1782 | 1783 | 1784 | 1780 | 1779 | 1776 | 1775 | 1772 | 1773 | 1770 | 1769 | 1768 | 1767 | 1763 | 1765 | 1766 | 1762 | 1760 | 1761 | 1757 | 1758 | 1759 | 1755 | 1749 | 1750 | 1751 | 1752 | 1753 | 1754 | 1748 | 1747 | 1745 | 1744 | 1742 | 1743 | 1740 | 1736 | 1737 | 1735 | 1733 | 1732 | 1729 | 1722 | 1723 | 1716 | 1717 | 1718 | 1715 | 1714 | 1712 | 1713 | 1711 | 1710 | 1709 | 1708 | 1706 | 1705 | 1699 | 1700 | 1701 | 1702 | 1703 | 1704 | 1693 | 1694 | 1695 | 1696 | 1697 | 1692 | 1687 | 1690 | 1691 | 1685 | 1686 | 1683 | 1684 | 1682 | 1681 | 1679 | 1677 | 1678 | 1675 | 1674 | 1671 | 1672 | 1669 | 1668 | 1665 | 1666 | 1667 | 1663 | 1662 | 1659 | 1658 | 1657 | 1654 | 1655 | 1656 | 1650 | 1647 | 1648 | 1649 | 1638 | 1637 | 1636 | 1635 | 1628 | 1623 | 1625 | 1626 | 1627 | 1618 | 1619 | 1622 | 1614 | 1615 | 1616 | 1617 | 1613 | 1603 | 1606 | 1607 | 1608 | 1609 | 1611 | 1612 | 1591 | 1592 | 1593 | 1594 | 1595 | 1596 | 1597 | 1598 | 1599 | 1600 | 1602 | 1578 | 1579 | 1580 | 1581 | 1582 | 1583 | 1584 | 1585 | 1586 | 1587 | 1588 | 1589 | 1590 | 1576 | 1577 | 1575 | 1574 | 1573 | 1288 | 1570 | 1565 | 1566 | 1567 | 1568 | 1564 | 1560 | 1559 | 1555 | 1556 | 1557 | 1558 | 1551 | 1553 | 1554 | 1548 | 1549 | 1550 | 1547 | 1545 | 1546 | 1543 | 1544 | 1537 | 1538 | 1542 | 1533 | 1531 | 1529 | 1528 | 1525 | 1526 | 1527 | 1523 | 1524 | 1521 | 1520 | 1517 | 1518 | 1519 | 1515 | 1516 | 1509 | 1510 | 1511 | 1504 | 1505 | 1506 | 1507 | 1508 | 1499 | 1500 | 1501 | 1502 | 1503 | 1497 | 1498 | 1493 | 1494 | 1495 | 1496 | 1489 | 1488 | 1487 | 1485 | 1484 | 1479 | 1481 | 1483 | 1621 | 1477 | 1476 | 1472 | 1473 | 1471 | 1470 | 1468 | 1469 | 1467 | 1454 | 1457 | 1458 | 1459 | 1460 | 1461 | 1462 | 1463 | 1452 | 1451 | 1446 | 1447 | 1448 | 1449 | 1450 | 1442 | 1443 | 1432 | 1435 | 1436 | 1437 | 1439 | 1396 | 1399 | 1401 | 1402 | 1403 | 1404 | 1405 | 1407 | 1408 | 1409 | 1410 | 1411 | 1412 | 1413 | 1414 | 1418 | 1419 | 1420 | 1421 | 1422 | 1423 | 1424 | 1425 | 1426 | 1427 | 1429 | 1430 | 1341 | 1342 | 1343 | 1344 | 1391 | 1392 | 1393 | 1394 | 1339 | 1340 | 1337 | 1329 | 1330 | 1331 | 1332 | 1333 | 1335 | 1328 | 1327 | 1321 | 1322 | 1323 | 1324 | 1325 | 1320 | 1301 | 1302 | 1303 | 1304 | 1305 | 1306 | 1307 | 1308 | 1309 | 1310 | 1311 | 1312 | 1313 | 1314 | 1315 | 1297 | 1298 | 1299 | 1300 | 1291 | 1292 | 1293 | 1295 | 1296 | 1290 | 1280 | 1281 | 1282 | 1285 | 1286 | 1287 | 1279 | 1276 | 1277 | 1278 | 1275 | 1264 | 1265 | 1266 | 1268 | 1269 | 1270 | 1271 | 1272 | 1273 | 1261 | 1262 | 1259 | 1260 | 1257 | 1258 | 1255 | 1254 | 1252 | 1250 | 1249 | 1247 | 1243 | 1244 | 1245 | 1246 | 1241 | 1242 | 1240 | 1238 | 1239 | 1237 | 1236 | 1235 | 1231 | 1232 | 1233 | 1234 | 1228 | 1229 | 1230 | 1224 | 1225 | 1226 | 1223 | 1220 | 1221 | 1222 | 1215 | 1216 | 1217 | 1218 | 1211 | 1212 | 1213 | 1214 | 1209 | 1210 | 1208 | 1202 | 1204 | 1205 | 1206 | 1200 | 1201 | 1199 | 1196 | 1198 | 1192 | 1193 | 1189 | 1190 | 1191 | 1185 | 1178 | 1179 | 1182 | 1184 | 1166 | 1167 | 1168 | 1169 | 1171 | 1173 | 1174 | 1164 | 1163 | 1153 | 1154 | 1155 | 1156 | 1157 | 1158 | 1159 | 1160 | 1161 | 1151 | 1152 | 1147 | 1148 | 1149 | 1146 | 1142 | 1143 | 1144 | 1145 | 1138 | 1139 | 1140 | 1136 | 1133 | 1134 | 1135 | 1132 | 629 | 1130 | 1131 | 1129 | 1123 | 1124 | 1125 | 1126 | 1127 | 1128 | 1122 | 1121 | 1120 | 1119 | 1116 | 1117 | 1118 | 1115 | 1114 | 1109 | 1111 | 1112 | 1113 | 1107 | 1106 | 1099 | 1100 | 1101 | 1102 | 1103 | 1098 | 1094 | 1095 | 1097 | 1093 | 1091 | 1092 | 1089 | 1090 | 1088 | 1085 | 1086 | 1081 | 1082 | 1078 | 1079 | 1080 | 1076 | 1077 | 1075 | 1074 | 743 | 1072 | 1073 | 1070 | 1071 | 1069 | 1068 | 1067 | 1057 | 1058 | 1059 | 1060 | 1061 | 1062 | 1063 | 1064 | 1065 | 1066 | 1055 | 730 | 1047 | 1048 | 1049 | 1050 | 1051 | 1052 | 1053 | 1042 | 1043 | 1044 | 1045 | 1046 | 1036 | 1037 | 1038 | 1039 | 1040 | 1041 | 1034 | 1035 | 910 | 1032 | 935 | 1030 | 1031 | 1026 | 1027 | 1028 | 1029 | 1024 | 1025 | 1023 | 1021 | 1022 | 1018 | 1019 | 1020 | 1017 | 684 | 1016 | 1015 | 890 | 1014 | 1011 | 1012 | 1013 | 1010 | 1009 | 1008 | 1007 | 660 | 1006 | 690 | 1005 | 1002 | 1003 | 997 | 999 | 1000 | 1001 | 996 | 995 | 994 | 987 | 988 | 989 | 990 | 991 | 992 | 984 | 985 | 986 | 431 | 983 | 982 | 979 | 980 | 981 | 961 | 977 | 978 | 975 | 976 | 972 | 974 | 969 | 970 | 971 | 968 | 911 | 967 | 817 | 850 | 853 | 658 | 659 | 439 | 966 | 964 | 962 | 963 | 960 | 958 | 959 | 957 | 954 | 955 | 956 | 952 | 953 | 949 | 950 | 951 | 947 | 948 | 946 | 945 | 944 | 943 | 942 | 941 | 938 | 936 | 937 | 934 | 931 | 932 | 933 | 752 | 292 | 815 | 816 | 819 | 316 | 832 | 839 | 846 | 847 | 854 | 855 | 863 | 864 | 865 | 362 | 879 | 888 | 891 | 918 | 689 | 716 | 722 | 724 | 741 | 744 | 746 | 749 | 750 | 929 | 927 | 928 | 925 | 926 | 924 | 153 | 923 | 919 | 920 | 921 | 916 | 914 | 912 | 908 | 909 | 905 | 906 | 464 | 354 | 904 | 878 | 900 | 893 | 894 | 895 | 896 | 897 | 892 | 898 | 899 | 889 | 351 | 885 | 886 | 880 | 881 | 883 | 884 | 667 | 874 | 875 | 361 | 930 | 940 | 430 | 434 | 873 | 825 | 826 | 828 | 829 | 844 | 845 | 849 | 852 | 856 | 857 | 858 | 859 | 860 | 870 | 697 | 764 | 862 | 861 | 818 | 851 | 663 | 830 | 831 | 833 | 834 | 835 | 836 | 838 | 840 | 842 | 843 | 824 | 837 | 822 | 820 | 801 | 810 | 811 | 812 | 814 | 628 | 656 | 657 | 661 | 664 | 665 | 666 | 668 | 669 | 670 | 674 | 675 | 677 | 678 | 680 | 681 | 682 | 683 | 685 | 686 | 687 | 688 | 691 | 692 | 693 | 694 | 696 | 698 | 699 | 700 | 701 | 702 | 703 | 704 | 705 | 713 | 459 | 717 | 719 | 720 | 721 | 725 | 729 | 731 | 734 | 736 | 737 | 740 | 748 | 751 | 754 | 755 | 756 | 757 | 758 | 759 | 760 | 761 | 762 | 711 | 813 | 809 | 808 | 803 | 804 | 805 | 364 | 802 | 800 | 798 | 796 | 797 | 795 | 791 | 792 | 793 | 794 | 461 | 790 | 787 | 788 | 770 | 771 | 772 | 773 | 774 | 775 | 777 | 782 | 784 | 768 | 769 | 767 | 765 | 766 | 626 | 726 | 727 | 728 | 710 | 706 | 295 | 444 | 484 | 652 | 654 | 655 | 643 | 646 | 647 | 648 | 649 | 650 | 630 | 631 | 633 | 634 | 635 | 638 | 639 | 640 | 564 | 578 | 579 | 582 | 583 | 584 | 587 | 588 | 590 | 591 | 592 | 593 | 594 | 595 | 596 | 597 | 598 | 599 | 600 | 601 | 602 | 603 | 604 | 605 | 606 | 607 | 608 | 609 | 610 | 611 | 613 | 614 | 615 | 616 | 617 | 618 | 619 | 620 | 623 | 438 | 442 | 443 | 447 | 448 | 455 | 465 | 466 | 472 | 473 | 481 | 482 | 483 | 576 | 575 | 562 | 532 | 535 | 537 | 539 | 541 | 543 | 545 | 547 | 551 | 553 | 555 | 513 | 514 | 515 | 516 | 517 | 518 | 519 | 520 | 521 | 522 | 523 | 524 | 525 | 526 | 527 | 528 | 530 | 500 | 501 | 502 | 503 | 504 | 505 | 506 | 507 | 508 | 509 | 511 | 487 | 488 | 489 | 491 | 492 | 495 | 496 | 499 | 458 | 456 | 360 | 294 | 293 | 415 | 416 | 404 | 402 | 398 | 401 | 377 | 386 | 372 | 369 | 368 | 358 | 344 | 353 | 355 | 321 | 322 | 325 | 319 | 257 | 8 | 13 | 14 | 271 | 272 | 33 | 289 | 34 | 35 | 296 | 44 | 45 | 86 | 98 | 100 | 106 | 117 | 139 | 145 | 159 | 182 | 183 | 184 | 185 | 210 | 211 | 212 | 216 | 222 | 223 | 235 | 239 | 240 | 243 | 246 | 248 | 250 | 3587 | 3590 | 3160

High-titanium glazes:

Great on a test tile, troublesome on ware

On this M390 red clay test tile, the titanium-variegated cone 6 calcia matte glaze G1214Z1 looks excellent (rutile has a similar effect). But that appearance depends on a combination of factors: glaze chemistry, 5% titanium dioxide, the titanium grade, application thickness, the red M390 body and the PLC6DS firing schedule. The relief of the tile especially flatters it - forcing the glaze thin over high points and allowing it to pool in recesses, displaying a whole range of effects in just a few centimetres.

The tile tells you what effects a glaze is capable of; it does not necessarily tell you what the glaze will look like on ware. These mugs demonstrate that. They were fired using the C6DHSC schedule and are made from buff-burning M340 (left) and M390. The mug on the right also has a heavier, less-even application. Surprisingly, some of the thickest runs become more transparent rather than more opaque. That is a reminder that the pale, variegated character of this glaze is not simply the result of titanium acting as an opacifier; it depends heavily on melt thickness and titanium-driven crystallization during cooling.

A titanium opacified glaze on a mug

Related Pictures

Titanium Dioxide in a cone 6 calcia matte glaze


Titainium glaze sample tile

This picture has its own page with more detail, click here to see it.

The glaze is G1214Z1 cone 6 base calcia matte on Plainsman M390 fired at cone 6 using the PLC6DS schedule. 5% titanium dioxide has been added (a high percentage). Titanium can create reactive glazes, like rutile, with no other colorants added. This effect also works well on matte surfaces, but the glaze needs good melt fluidity (that is good because functional mattes melt well). Calcia mattes host crystallization and work particularly well. Because titanium dioxide does not contain iron oxide, lighter colors and better blues are possible compared to rutile (iron is still needed, but it is coming from the body here). Like rutile, the effects are dependent on the cooling rate of the firing, slower cools produce more reactivity. Even application without drips is important (mixing as a thixotropic dipping glaze is best). This appearance also depends on using a dark-burning body or engobe.

Rutile in functional glazes:

Push the limit and you might get this


Rutile saturated glazes

This picture has its own page with more detail, click here to see it.

The 80:20 GA6-A Alberta Slip base becomes oatmeal-like when oversaturated with rutile and/or titanium (left: 6% rutile + 3% titanium dioxide; right: 4% rutile + 2% titanium dioxide). The rough surface results from excessive crystallization of titanium-bearing phases from the melt during cooling. It is unpleasant to touch, readily shows cutlery marking and is less desirable for functional surfaces. In glazes of this type, rutile additions above about 4% can become increasingly difficult to keep smooth and consistent. Crystallization, rather than phase separation, increasingly dominates the variegation mechanism.

One way of avoiding problems is staying below the tipping point, keeping the percentage as low as possible while still getting the desired variegation (of course, that will vary depending on the melt fluidity of the glaze and kiln cooling). Surprisingly, making the glaze more fluid does not necessarily solve the problem. Greater melt fluidity increases ion mobility and can actually promote crystal growth during cooling, producing an even rougher surface.

Links

Materials Titanium Dioxide
A super white powder used in ceramic glazes to variegate, opacify and moderate color.
Glossary Opacifier
Glaze opacity refers to the degree to which it is opaque. Opacifiers are powders added to transparent ceramic glazes to make them opaque.
Glossary Glaze laydown
Refers to the quality of the dried ceramic glaze layer and how this affects the fired result: e.g. density, hardness, evenness, thickness, freedom from defects, etc.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy