3899 | 3898 | 3897 | 3896 | 3890 | 3891 | 3892 | 3888 | 3889 | 3883 | 3885 | 3882 | 3880 | 3881 | 3878 | 3877 | 3876 | 3871 | 3872 | 3874 | 3869 | 3870 | 3866 | 3867 | 3864 | 3863 | 3862 | 3861 | 3860 | 3859 | 3838 | 3857 | 3858 | 3855 | 3856 | 3851 | 3853 | 3854 | 3849 | 3850 | 3852 | 3846 | 3848 | 3843 | 3840 | 3841 | 3842 | 3837 | 3836 | 3833 | 3831 | 3832 | 3829 | 3827 | 3828 | 3826 | 3824 | 3823 | 3822 | 3820 | 3819 | 3818 | 3815 | 3816 | 3817 | 3814 | 3813 | 3811 | 3810 | 3806 | 3807 | 3808 | 3805 | 3803 | 3802 | 3801 | 3800 | 3797 | 3798 | 3796 | 3793 | 3794 | 3792 | 3789 | 3786 | 3784 | 3787 | 3781 | 3779 | 3775 | 3773 | 3774 | 3772 | 3767 | 3768 | 3769 | 3762 | 3760 | 3759 | 3755 | 3752 | 3753 | 3754 | 3750 | 3748 | 3749 | 3742 | 3743 | 3745 | 3746 | 3747 | 3740 | 3737 | 3738 | 3739 | 3736 | 3734 | 3733 | 3732 | 3731 | 3729 | 3728 | 3726 | 3725 | 3724 | 3723 | 3721 | 3719 | 3720 | 3718 | 3716 | 3713 | 3712 | 3711 | 3710 | 3709 | 3707 | 3708 | 3706 | 3705 | 3704 | 3702 | 3701 | 3700 | 3699 | 3698 | 3695 | 3696 | 3697 | 3692 | 3693 | 3694 | 3690 | 3691 | 3689 | 3688 | 3685 | 3686 | 3679 | 3678 | 3676 | 3675 | 3674 | 3672 | 3673 | 3663 | 3664 | 3661 | 3656 | 3657 | 3658 | 3659 | 3651 | 3652 | 3654 | 3655 | 3650 | 3649 | 3648 | 3646 | 3647 | 3644 | 3645 | 3643 | 3642 | 3640 | 3639 | 3637 | 3636 | 3634 | 3635 | 3632 | 3631 | 3629 | 3630 | 3626 | 3627 | 3624 | 3625 | 3622 | 3623 | 3620 | 3619 | 3612 | 3610 | 3611 | 3606 | 3607 | 3608 | 3609 | 3602 | 3603 | 3604 | 3605 | 3601 | 3600 | 3599 | 3598 | 3596 | 3595 | 3594 | 3593 | 3591 | 3592 | 3588 | 3589 | 3585 | 3586 | 3584 | 3580 | 3581 | 3582 | 3583 | 3579 | 3577 | 3578 | 3576 | 3574 | 3572 | 3573 | 3571 | 3570 | 3568 | 3567 | 3565 | 3562 | 3563 | 3560 | 3561 | 3559 | 3557 | 3556 | 3555 | 3554 | 3553 | 3551 | 3552 | 3550 | 3549 | 3548 | 3547 | 3546 | 3544 | 3545 | 3543 | 3542 | 3538 | 3539 | 3540 | 3541 | 3536 | 3537 | 3535 | 3534 | 3531 | 3532 | 3533 | 3529 | 3530 | 3527 | 3528 | 3526 | 3525 | 3524 | 3523 | 3522 | 3520 | 3518 | 3516 | 3517 | 3515 | 3514 | 3512 | 3513 | 3511 | 3510 | 3509 | 3508 | 3507 | 3506 | 3505 | 3504 | 3046 | 3503 | 3493 | 3494 | 3490 | 3491 | 3486 | 3489 | 3485 | 3481 | 3483 | 3492 | 3479 | 3480 | 3476 | 3477 | 3474 | 3473 | 3471 | 3470 | 3469 | 3468 | 3465 | 3466 | 3467 | 3463 | 3459 | 3460 | 3461 | 3462 | 3458 | 3457 | 3456 | 3455 | 3454 | 3452 | 3449 | 3448 | 3447 | 3446 | 3445 | 3443 | 3444 | 3442 | 3441 | 3439 | 3440 | 3437 | 3438 | 3435 | 3436 | 3431 | 3433 | 3434 | 3430 | 3427 | 3428 | 3425 | 3426 | 3423 | 3422 | 3419 | 3421 | 3418 | 3415 | 3416 | 3417 | 3414 | 3413 | 3411 | 3412 | 3409 | 3410 | 3408 | 3401 | 3402 | 3403 | 3404 | 3406 | 3407 | 3400 | 3399 | 3397 | 3393 | 3394 | 3396 | 3392 | 3391 | 3387 | 3389 | 3390 | 3385 | 3384 | 3383 | 3382 | 3379 | 3380 | 3381 | 3378 | 3376 | 3375 | 3374 | 3373 | 3372 | 3370 | 3367 | 3368 | 3369 | 3364 | 3363 | 3360 | 3359 | 3358 | 3356 | 3355 | 3354 | 3352 | 3349 | 3348 | 3347 | 3344 | 3345 | 3346 | 3343 | 3342 | 3340 | 3338 | 3339 | 3337 | 3335 | 3336 | 3334 | 3333 | 3330 | 3322 | 3319 | 3320 | 3321 | 3317 | 3316 | 3313 | 3314 | 3315 | 3312 | 3310 | 3311 | 3309 | 3307 | 3308 | 3306 | 3304 | 3303 | 3302 | 3300 | 3301 | 3298 | 3299 | 3296 | 3295 | 3293 | 3294 | 3292 | 3291 | 3290 | 3289 | 3288 | 3286 | 3285 | 3284 | 3280 | 3281 | 3282 | 3278 | 3277 | 3272 | 3273 | 3274 | 3275 | 3276 | 3271 | 3270 | 3267 | 3268 | 3265 | 3266 | 3264 | 3262 | 3261 | 3260 | 3259 | 3258 | 3257 | 3256 | 3255 | 3253 | 3254 | 3251 | 3248 | 3247 | 3245 | 3246 | 3244 | 3241 | 3239 | 3236 | 3237 | 3235 | 3234 | 3233 | 3231 | 3232 | 3230 | 3229 | 3201 | 3202 | 3203 | 3204 | 3205 | 3206 | 3207 | 3208 | 3209 | 3210 | 3211 | 3212 | 3213 | 3214 | 3215 | 3216 | 3217 | 3219 | 3220 | 3222 | 3223 | 3224 | 3226 | 3227 | 3228 | 3199 | 3198 | 3197 | 3195 | 3196 | 3191 | 3192 | 3193 | 3194 | 3188 | 3189 | 3187 | 3185 | 3186 | 3183 | 3181 | 3182 | 3179 | 3180 | 3177 | 3176 | 3175 | 3174 | 3173 | 3169 | 3167 | 3164 | 3162 | 3159 | 3158 | 3157 | 3154 | 3155 | 3156 | 3153 | 3149 | 3150 | 3144 | 3145 | 3146 | 3147 | 3148 | 3142 | 3143 | 3139 | 3141 | 3138 | 3136 | 3137 | 3132 | 3135 | 3131 | 3130 | 3127 | 3124 | 3125 | 3126 | 3122 | 3123 | 3121 | 3120 | 3117 | 3119 | 3116 | 3112 | 3113 | 3114 | 3109 | 3110 | 3111 | 3098 | 3099 | 3102 | 3103 | 3104 | 3105 | 3106 | 3107 | 3108 | 3096 | 3094 | 3095 | 3091 | 3092 | 3093 | 3089 | 3090 | 3087 | 3086 | 3082 | 3083 | 3084 | 3080 | 3081 | 3079 | 3078 | 3077 | 3074 | 3075 | 3076 | 3073 | 3072 | 3070 | 3053 | 3055 | 3056 | 3057 | 3058 | 3059 | 3060 | 3061 | 3062 | 3063 | 3064 | 3065 | 3066 | 3067 | 3068 | 3069 | 3052 | 3050 | 3051 | 3048 | 3049 | 3047 | 3044 | 3043 | 3042 | 3041 | 3040 | 3038 | 3039 | 3037 | 3036 | 3035 | 3034 | 3033 | 3029 | 3030 | 3031 | 3023 | 3024 | 3021 | 3022 | 3019 | 3016 | 3017 | 3018 | 3015 | 3012 | 3013 | 3014 | 3011 | 3010 | 3007 | 3008 | 3009 | 3005 | 3006 | 3004 | 3001 | 3002 | 3003 | 2999 | 2995 | 2996 | 2994 | 2991 | 2992 | 2993 | 2990 | 2989 | 2986 | 2987 | 2988 | 2982 | 2983 | 2984 | 2985 | 2979 | 2980 | 2976 | 2977 | 2974 | 2973 | 2970 | 2971 | 2967 | 2968 | 2969 | 2966 | 2964 | 2965 | 2963 | 2961 | 2962 | 2960 | 2958 | 2952 | 2953 | 2954 | 2955 | 2956 | 2950 | 2951 | 2948 | 2949 | 2945 | 2946 | 2947 | 2944 | 2943 | 2939 | 2940 | 2941 | 2942 | 2937 | 2938 | 2936 | 2935 | 2929 | 2930 | 2931 | 2932 | 2933 | 2934 | 2928 | 2927 | 2925 | 2926 | 2921 | 2922 | 2923 | 2924 | 2919 | 2920 | 2917 | 2918 | 2915 | 2916 | 2913 | 2914 | 2912 | 2911 | 2910 | 2909 | 2907 | 2908 | 2906 | 2905 | 2903 | 2904 | 2900 | 2899 | 2898 | 2893 | 2894 | 2895 | 2896 | 2897 | 2890 | 2891 | 2892 | 2887 | 2888 | 2889 | 2885 | 2882 | 2883 | 2884 | 2880 | 2881 | 2878 | 2877 | 2872 | 2873 | 2874 | 2875 | 2876 | 2871 | 2868 | 2869 | 2870 | 2866 | 2867 | 2865 | 2864 | 2862 | 2863 | 2861 | 2860 | 2858 | 2859 | 2856 | 2857 | 2854 | 2855 | 2853 | 2852 | 2848 | 2849 | 2850 | 2847 | 2845 | 2846 | 2843 | 2842 | 2840 | 2841 | 2839 | 2838 | 2837 | 2836 | 2835 | 2833 | 2834 | 2832 | 2831 | 2828 | 2829 | 2827 | 2826 | 2825 | 2824 | 2822 | 2823 | 2820 | 2821 | 2819 | 2816 | 2815 | 2814 | 2813 | 2812 | 2811 | 2793 | 2794 | 2795 | 2796 | 2797 | 2798 | 2799 | 2800 | 2801 | 2802 | 2803 | 2804 | 2805 | 2806 | 2807 | 2808 | 2809 | 2810 | 2791 | 2792 | 2790 | 2787 | 2788 | 2784 | 2785 | 2786 | 2781 | 2782 | 2780 | 2777 | 2778 | 2779 | 2776 | 2775 | 2774 | 2772 | 2771 | 2769 | 2770 | 2768 | 2767 | 2766 | 2764 | 2765 | 2762 | 2763 | 2761 | 2760 | 2759 | 2758 | 2756 | 2752 | 2753 | 2754 | 2755 | 2750 | 2751 | 2748 | 2749 | 2747 | 2745 | 2746 | 2742 | 2743 | 2740 | 2741 | 2739 | 2737 | 2738 | 2736 | 2735 | 2734 | 2733 | 2732 | 2729 | 2730 | 2731 | 2728 | 2727 | 2726 | 2723 | 2724 | 2725 | 2722 | 2719 | 2720 | 2721 | 2718 | 2716 | 2715 | 2714 | 2713 | 2712 | 2711 | 2709 | 2708 | 2706 | 2707 | 2704 | 2705 | 2703 | 2702 | 2700 | 2693 | 2694 | 2695 | 2696 | 2697 | 2698 | 2699 | 2692 | 2690 | 2691 | 2689 | 2688 | 2687 | 2686 | 2685 | 2684 | 2683 | 2680 | 2681 | 2682 | 2678 | 2679 | 2677 | 2676 | 2675 | 2674 | 2673 | 2672 | 2671 | 2670 | 2669 | 2666 | 2668 | 2664 | 2665 | 2662 | 2663 | 2660 | 2661 | 2656 | 2657 | 2658 | 2659 | 2655 | 2654 | 2653 | 2652 | 2649 | 2650 | 2651 | 2646 | 2647 | 2648 | 2643 | 2644 | 2641 | 2642 | 2639 | 2640 | 2637 | 2638 | 2635 | 2636 | 2633 | 2634 | 2631 | 2632 | 2630 | 2629 | 2627 | 2628 | 2624 | 2626 | 2621 | 2622 | 2623 | 2618 | 2619 | 2617 | 2614 | 2615 | 2616 | 2613 | 2612 | 2607 | 2608 | 2609 | 2611 | 2606 | 2605 | 2602 | 2603 | 2604 | 2600 | 2601 | 2599 | 2598 | 2597 | 2595 | 2596 | 2591 | 2592 | 2593 | 2594 | 2585 | 2586 | 2587 | 2588 | 2589 | 2590 | 2584 | 2583 | 2582 | 2581 | 2578 | 2580 | 2576 | 2577 | 2573 | 2574 | 2575 | 2572 | 2571 | 2566 | 2567 | 2569 | 2570 | 2563 | 2565 | 2562 | 2561 | 2560 | 2558 | 2559 | 2557 | 2556 | 2554 | 2555 | 2551 | 2552 | 2548 | 2549 | 2550 | 2547 | 2545 | 2546 | 2542 | 2543 | 2544 | 2540 | 2541 | 2539 | 2537 | 2536 | 2533 | 2534 | 2535 | 2531 | 2532 | 2530 | 2528 | 2525 | 2526 | 2527 | 2522 | 2523 | 2521 | 2519 | 2520 | 2518 | 2517 | 2516 | 2515 | 2514 | 2513 | 2511 | 2512 | 2509 | 2510 | 2508 | 2506 | 2507 | 2505 | 2504 | 2503 | 2502 | 2501 | 2499 | 2490 | 2494 | 2495 | 2496 | 2497 | 2498 | 2489 | 2488 | 2487 | 2486 | 2485 | 2484 | 2483 | 2482 | 2481 | 2479 | 2480 | 2478 | 2474 | 2475 | 2476 | 2477 | 2472 | 2473 | 2471 | 2470 | 2465 | 2466 | 2467 | 2468 | 2469 | 2464 | 2461 | 2460 | 2459 | 2458 | 2457 | 2454 | 2455 | 2456 | 2451 | 2452 | 2453 | 2449 | 2450 | 2447 | 2448 | 2442 | 2443 | 2444 | 2445 | 2446 | 2440 | 2441 | 2439 | 2436 | 2437 | 2438 | 2434 | 2435 | 2433 | 2432 | 2429 | 2430 | 2431 | 2425 | 2426 | 2427 | 2428 | 2422 | 2423 | 2424 | 2421 | 2417 | 2418 | 2419 | 2420 | 2416 | 2415 | 2412 | 2411 | 2410 | 2408 | 2409 | 2407 | 2406 | 2405 | 2403 | 2404 | 2402 | 2401 | 2400 | 2399 | 2398 | 2397 | 2396 | 2395 | 2394 | 2392 | 2393 | 2390 | 2389 | 2387 | 2386 | 2385 | 2384 | 2383 | 2380 | 2375 | 2376 | 2377 | 2378 | 2379 | 2374 | 2373 | 2372 | 2371 | 2369 | 2370 | 2366 | 2368 | 2361 | 2362 | 2363 | 2364 | 2365 | 2360 | 2359 | 2355 | 2356 | 2357 | 2354 | 2353 | 2350 | 2351 | 2348 | 2349 | 2346 | 2347 | 2344 | 2345 | 2343 | 2342 | 2341 | 2337 | 2339 | 2340 | 2335 | 2336 | 2334 | 2333 | 2328 | 2329 | 2330 | 2331 | 2332 | 2327 | | 2323 | 2324 | 2325 | 2322 | 2321 | 2316 | 2317 | 2318 | 2319 | 2320 | 2314 | 2315 | 2311 | 2312 | 2313 | 2309 | 2308 | 2306 | 2307 | 2304 | 2305 | 2303 | 2299 | 2300 | 2301 | 2297 | 2294 | 2295 | 2296 | 2292 | 2278 | 2279 | 2280 | 2282 | 2283 | 2284 | 2285 | 2286 | 2287 | 2288 | 2289 | 2290 | 2273 | 2274 | 2275 | 2276 | 2277 | 2271 | 2270 | 2269 | 2266 | 2265 | 2263 | 2264 | 2262 | 2260 | 2261 | 2259 | 2258 | 2257 | 2255 | 2256 | 2254 | 2250 | 2252 | 2249 | 2247 | 2248 | 2246 | 2242 | 2243 | 2245 | 2239 | 2240 | 2241 | 2235 | 2236 | 2237 | 2238 | 2234 | 2233 | 2232 | 2231 | 2230 | 2229 | 2225 | 2226 | 2224 | 2222 | 2223 | 2220 | 2221 | 2218 | 2219 | 2216 | 2217 | 2214 | 2215 | 2213 | 2211 | 2212 | 2210 | 2209 | 2208 | 2207 | 2206 | 2205 | 2203 | 2204 | 2202 | 2201 | 2199 | 2200 | 2198 | 2197 | 2195 | 2196 | 2194 | 2192 | 2193 | 2191 | 2189 | 2190 | 2188 | 2186 | 2187 | 2185 | 2184 | 2182 | 2183 | 2180 | 2178 | 2179 | 2176 | 2177 | 2172 | 2173 | 2174 | 2175 | 2171 | 2166 | 2167 | 2169 | 2170 | 2165 | 2156 | 2157 | 2158 | 2159 | 2161 | 2162 | 2164 | 2153 | 2154 | 2155 | 2151 | 2150 | 2148 | 2149 | 2142 | 2143 | 2144 | 2145 | 2146 | 2147 | 2140 | 2141 | 2138 | 2139 | 2136 | 2137 | 2135 | 2129 | 2130 | 2131 | 2132 | 2133 | 2134 | 2128 | 2127 | 2126 | 2125 | 2124 | 2121 | 2122 | 2123 | 2118 | 2117 | 2115 | 2116 | 2114 | 2113 | 2112 | 2111 | 2109 | 2108 | 2107 | 2106 | 2104 | 2105 | 2101 | 2102 | 2103 | 2099 | 2100 | 2096 | 2094 | 2095 | 2093 | 2092 | 2091 | 2089 | 2090 | 2088 | 2087 | 2086 | 2085 | 2084 | 2082 | 2083 | 2081 | 2078 | 2079 | 2080 | 2076 | 2077 | 2073 | 2074 | 2075 | 2071 | 2069 | 2066 | 2067 | 2068 | 2064 | 2060 | 2061 | 2062 | 2059 | 2057 | 2058 | 2052 | 2053 | 2054 | 2055 | 2056 | 2049 | 2050 | 2051 | 2048 | 2047 | 2046 | 2042 | 2043 | 2044 | 2045 | 2040 | 2039 | 2038 | 2036 | 2035 | 2029 | 2030 | 2031 | 2033 | 2034 | 2027 | 2024 | 2025 | 2026 | 2017 | 2018 | 2019 | 2020 | 2021 | 2022 | 2016 | 2015 | 2014 | 2013 | 2010 | 2011 | 2012 | 2008 | 2009 | 2007 | 2001 | 2002 | 2003 | 2004 | 2005 | 1993 | 1995 | 1998 | 2000 | 1990 | 1991 | 1987 | 1988 | 1986 | 1983 | 1984 | 1976 | 1977 | 1978 | 1979 | 1980 | 1981 | 1974 | 1975 | 1973 | 1972 | 1970 | 1968 | 1969 | 1967 | 1966 | 1965 | 1964 | 1962 | 1961 | 1959 | 1960 | 1955 | 1956 | 1957 | 1954 | 1952 | 1953 | 1950 | 1951 | 1948 | 1947 | 1946 | 1944 | 1945 | 1940 | 1941 | 1942 | 1943 | 1939 | 1934 | 1935 | 1936 | 1937 | 1938 | 1932 | 1933 | 1931 | 1930 | 1928 | 1927 | 1922 | 1923 | 1924 | 1925 | 1926 | 1916 | 1918 | 1919 | 1920 | 1921 | 1915 | 1914 | 1906 | 1907 | 1908 | 1909 | 1910 | 1911 | 1912 | 1913 | 1902 | 1904 | 1905 | 1895 | 1896 | 1897 | 1899 | 1900 | 1901 | 1891 | 1893 | 1894 | 1890 | 1888 | 1889 | 1887 | 1885 | 1882 | 1883 | 1884 | 1874 | 1875 | 1876 | 1877 | 1878 | 1879 | 1870 | 1871 | 1872 | 1873 | 1868 | 1867 | 1866 | 1865 | 1864 | 1858 | 1859 | 1860 | 1861 | 1862 | 1863 | 1854 | 1855 | 1850 | 1851 | 1852 | 1848 | 1849 | 1846 | 1847 | 1843 | 1844 | 1845 | 1842 | 1831 | 1832 | 1833 | 1834 | 1835 | 1836 | 1838 | 1839 | 1840 | 1841 | 1828 | 1829 | 1830 | 1827 | 1826 | 1825 | 1823 | 1824 | 1818 | 1819 | 1820 | 1821 | 1822 | 1817 | 1815 | 1816 | 1814 | 1812 | 1811 | 1809 | 1810 | 1807 | 1806 | 1805 | 1804 | 1803 | 1802 | 1796 | 1797 | 1798 | 1799 | 1800 | 1801 | 1792 | 1793 | 1794 | 1791 | 1790 | 1789 | 1788 | 1786 | 1785 | 1781 | 1782 | 1783 | 1784 | 1780 | 1779 | 1776 | 1775 | 1772 | 1773 | 1770 | 1769 | 1768 | 1767 | 1763 | 1765 | 1766 | 1762 | 1760 | 1761 | 1757 | 1758 | 1759 | 1755 | 1749 | 1750 | 1751 | 1752 | 1753 | 1754 | 1748 | 1747 | 1745 | 1744 | 1742 | 1743 | 1740 | 1736 | 1737 | 1735 | 1733 | 1732 | 1729 | 1722 | 1723 | 1716 | 1717 | 1718 | 1715 | 1714 | 1712 | 1713 | 1711 | 1710 | 1709 | 1708 | 1706 | 1705 | 1699 | 1700 | 1701 | 1702 | 1703 | 1704 | 1693 | 1694 | 1695 | 1696 | 1697 | 1692 | 1687 | 1690 | 1691 | 1685 | 1686 | 1683 | 1684 | 1682 | 1681 | 1679 | 1677 | 1678 | 1675 | 1674 | 1671 | 1672 | 1669 | 1668 | 1665 | 1666 | 1667 | 1663 | 1662 | 1659 | 1658 | 1657 | 1654 | 1655 | 1656 | 1650 | 1647 | 1648 | 1649 | 1638 | 1637 | 1636 | 1635 | 1628 | 1623 | 1625 | 1626 | 1627 | 1618 | 1619 | 1622 | 1614 | 1615 | 1616 | 1617 | 1613 | 1603 | 1606 | 1607 | 1608 | 1609 | 1611 | 1612 | 1591 | 1592 | 1593 | 1594 | 1595 | 1596 | 1597 | 1598 | 1599 | 1600 | 1602 | 1578 | 1579 | 1580 | 1581 | 1582 | 1583 | 1584 | 1585 | 1586 | 1587 | 1588 | 1589 | 1590 | 1576 | 1577 | 1575 | 1574 | 1573 | 1288 | 1570 | 1565 | 1566 | 1567 | 1568 | 1564 | 1560 | 1559 | 1555 | 1556 | 1557 | 1558 | 1551 | 1553 | 1554 | 1548 | 1549 | 1550 | 1547 | 1545 | 1546 | 1543 | 1544 | 1537 | 1538 | 1542 | 1533 | 1531 | 1529 | 1528 | 1525 | 1526 | 1527 | 1523 | 1524 | 1521 | 1520 | 1517 | 1518 | 1519 | 1515 | 1516 | 1509 | 1510 | 1511 | 1504 | 1505 | 1506 | 1507 | 1508 | 1499 | 1500 | 1501 | 1502 | 1503 | 1497 | 1498 | 1493 | 1494 | 1495 | 1496 | 1489 | 1488 | 1487 | 1485 | 1484 | 1479 | 1481 | 1483 | 1621 | 1477 | 1476 | 1472 | 1473 | 1471 | 1470 | 1468 | 1469 | 1467 | 1454 | 1457 | 1458 | 1459 | 1460 | 1461 | 1462 | 1463 | 1452 | 1451 | 1446 | 1447 | 1448 | 1449 | 1450 | 1442 | 1443 | 1432 | 1435 | 1436 | 1437 | 1439 | 1396 | 1399 | 1401 | 1402 | 1403 | 1404 | 1405 | 1407 | 1408 | 1409 | 1410 | 1411 | 1412 | 1413 | 1414 | 1418 | 1419 | 1420 | 1421 | 1422 | 1423 | 1424 | 1425 | 1426 | 1427 | 1429 | 1430 | 1341 | 1342 | 1343 | 1344 | 1391 | 1392 | 1393 | 1394 | 1339 | 1340 | 1337 | 1329 | 1330 | 1331 | 1332 | 1333 | 1335 | 1328 | 1327 | 1321 | 1322 | 1323 | 1324 | 1325 | 1320 | 1301 | 1302 | 1303 | 1304 | 1305 | 1306 | 1307 | 1308 | 1309 | 1310 | 1311 | 1312 | 1313 | 1314 | 1315 | 1297 | 1298 | 1299 | 1300 | 1291 | 1292 | 1293 | 1295 | 1296 | 1290 | 1280 | 1281 | 1282 | 1285 | 1286 | 1287 | 1279 | 1276 | 1277 | 1278 | 1275 | 1264 | 1265 | 1266 | 1268 | 1269 | 1270 | 1271 | 1272 | 1273 | 1261 | 1262 | 1259 | 1260 | 1257 | 1258 | 1255 | 1254 | 1252 | 1250 | 1249 | 1247 | 1243 | 1244 | 1245 | 1246 | 1241 | 1242 | 1240 | 1238 | 1239 | 1237 | 1236 | 1235 | 1231 | 1232 | 1233 | 1234 | 1228 | 1229 | 1230 | 1224 | 1225 | 1226 | 1223 | 1220 | 1221 | 1222 | 1215 | 1216 | 1217 | 1218 | 1211 | 1212 | 1213 | 1214 | 1209 | 1210 | 1208 | 1202 | 1204 | 1205 | 1206 | 1200 | 1201 | 1199 | 1196 | 1198 | 1192 | 1193 | 1189 | 1190 | 1191 | 1185 | 1178 | 1179 | 1182 | 1184 | 1166 | 1167 | 1168 | 1169 | 1171 | 1173 | 1174 | 1164 | 1163 | 1153 | 1154 | 1155 | 1156 | 1157 | 1158 | 1159 | 1160 | 1161 | 1151 | 1152 | 1147 | 1148 | 1149 | 1146 | 1142 | 1143 | 1144 | 1145 | 1138 | 1139 | 1140 | 1136 | 1133 | 1134 | 1135 | 1132 | 629 | 1130 | 1131 | 1129 | 1123 | 1124 | 1125 | 1126 | 1127 | 1128 | 1122 | 1121 | 1120 | 1119 | 1116 | 1117 | 1118 | 1115 | 1114 | 1109 | 1111 | 1112 | 1113 | 1107 | 1106 | 1099 | 1100 | 1101 | 1102 | 1103 | 1098 | 1094 | 1095 | 1097 | 1093 | 1091 | 1092 | 1089 | 1090 | 1088 | 1085 | 1086 | 1081 | 1082 | 1078 | 1079 | 1080 | 1076 | 1077 | 1075 | 1074 | 743 | 1072 | 1073 | 1070 | 1071 | 1069 | 1068 | 1067 | 1057 | 1058 | 1059 | 1060 | 1061 | 1062 | 1063 | 1064 | 1065 | 1066 | 1055 | 730 | 1047 | 1048 | 1049 | 1050 | 1051 | 1052 | 1053 | 1042 | 1043 | 1044 | 1045 | 1046 | 1036 | 1037 | 1038 | 1039 | 1040 | 1041 | 1034 | 1035 | 910 | 1032 | 935 | 1030 | 1031 | 1026 | 1027 | 1028 | 1029 | 1024 | 1025 | 1023 | 1021 | 1022 | 1018 | 1019 | 1020 | 1017 | 684 | 1016 | 1015 | 890 | 1014 | 1011 | 1012 | 1013 | 1010 | 1009 | 1008 | 1007 | 660 | 1006 | 690 | 1005 | 1002 | 1003 | 997 | 999 | 1000 | 1001 | 996 | 995 | 994 | 987 | 988 | 989 | 990 | 991 | 992 | 984 | 985 | 986 | 431 | 983 | 982 | 979 | 980 | 981 | 961 | 977 | 978 | 975 | 976 | 972 | 974 | 969 | 970 | 971 | 968 | 911 | 967 | 817 | 850 | 853 | 658 | 659 | 439 | 966 | 964 | 962 | 963 | 960 | 958 | 959 | 957 | 954 | 955 | 956 | 952 | 953 | 949 | 950 | 951 | 947 | 948 | 946 | 945 | 944 | 943 | 942 | 941 | 938 | 936 | 937 | 934 | 931 | 932 | 933 | 752 | 292 | 815 | 816 | 819 | 316 | 832 | 839 | 846 | 847 | 854 | 855 | 863 | 864 | 865 | 362 | 879 | 888 | 891 | 918 | 689 | 716 | 722 | 724 | 741 | 744 | 746 | 749 | 750 | 929 | 927 | 928 | 925 | 926 | 924 | 153 | 923 | 919 | 920 | 921 | 916 | 914 | 912 | 908 | 909 | 905 | 906 | 464 | 354 | 904 | 878 | 900 | 893 | 894 | 895 | 896 | 897 | 892 | 898 | 899 | 889 | 351 | 885 | 886 | 880 | 881 | 883 | 884 | 667 | 874 | 875 | 361 | 930 | 940 | 430 | 434 | 873 | 825 | 826 | 828 | 829 | 844 | 845 | 849 | 852 | 856 | 857 | 858 | 859 | 860 | 870 | 697 | 764 | 862 | 861 | 818 | 851 | 663 | 830 | 831 | 833 | 834 | 835 | 836 | 838 | 840 | 842 | 843 | 824 | 837 | 822 | 820 | 801 | 810 | 811 | 812 | 814 | 628 | 656 | 657 | 661 | 664 | 665 | 666 | 668 | 669 | 670 | 674 | 675 | 677 | 678 | 680 | 681 | 682 | 683 | 685 | 686 | 687 | 688 | 691 | 692 | 693 | 694 | 696 | 698 | 699 | 700 | 701 | 702 | 703 | 704 | 705 | 713 | 459 | 717 | 719 | 720 | 721 | 725 | 729 | 731 | 734 | 736 | 737 | 740 | 748 | 751 | 754 | 755 | 756 | 757 | 758 | 759 | 760 | 761 | 762 | 711 | 813 | 809 | 808 | 803 | 804 | 805 | 364 | 802 | 800 | 798 | 796 | 797 | 795 | 791 | 792 | 793 | 794 | 461 | 790 | 787 | 788 | 770 | 771 | 772 | 773 | 774 | 775 | 777 | 782 | 784 | 768 | 769 | 767 | 765 | 766 | 626 | 726 | 727 | 728 | 710 | 706 | 295 | 444 | 484 | 652 | 654 | 655 | 643 | 646 | 647 | 648 | 649 | 650 | 630 | 631 | 633 | 634 | 635 | 638 | 639 | 640 | 564 | 578 | 579 | 582 | 583 | 584 | 587 | 588 | 590 | 591 | 592 | 593 | 594 | 595 | 596 | 597 | 598 | 599 | 600 | 601 | 602 | 603 | 604 | 605 | 606 | 607 | 608 | 609 | 610 | 611 | 613 | 614 | 615 | 616 | 617 | 618 | 619 | 620 | 623 | 438 | 442 | 443 | 447 | 448 | 455 | 465 | 466 | 472 | 473 | 481 | 482 | 483 | 576 | 575 | 562 | 532 | 535 | 537 | 539 | 541 | 543 | 545 | 547 | 551 | 553 | 555 | 513 | 514 | 515 | 516 | 517 | 518 | 519 | 520 | 521 | 522 | 523 | 524 | 525 | 526 | 527 | 528 | 530 | 500 | 501 | 502 | 503 | 504 | 505 | 506 | 507 | 508 | 509 | 511 | 487 | 488 | 489 | 491 | 492 | 495 | 496 | 499 | 458 | 456 | 360 | 294 | 293 | 415 | 416 | 404 | 402 | 398 | 401 | 377 | 386 | 372 | 369 | 368 | 358 | 344 | 353 | 355 | 321 | 322 | 325 | 319 | 257 | 8 | 13 | 14 | 271 | 272 | 33 | 289 | 34 | 35 | 296 | 44 | 45 | 86 | 98 | 100 | 106 | 117 | 139 | 145 | 159 | 182 | 183 | 184 | 185 | 210 | 211 | 212 | 216 | 222 | 223 | 235 | 239 | 240 | 243 | 246 | 248 | 250 | 3587 | 3590 | 3160

A Super Plastic Stoneware Made With Two Materials

This mix showcases stoneware's advantages over porcelain

Left: 65% #6Tile kaolin and 35% nepheline syenite. Although it has great plasticity and fires white, it crazes the glaze and has 1% fired porosity (using the SHAB test).
Right: 65% M23 Old Hickory ball clay (similar to OM#4) and 35% nepheline syenite (feldspar would also work). The glaze fits, the body fires very dense (zero porosity) and plasticity is fantastic!
The body on the left needs a 20% silica addition (to stop the crazing) and more nepheline (to reduce porosity to porcelain levels). The remaining 40% kaolin will not be nearly enough for a workable plasticity (so bentonite will be needed). The body on the right does not need fixing; it works as is. Many feel that stoneware body recipes must be built on a feldspar-containing base clay having pottery plasticity (adding ball clay, kaolin, feldspar and silica and ending up with needlessly complicated recipes). But, ball clay is a base, all it needs is a non-plastic filler (to cut plasticity and therefore drying shrinkage) and a flux to vitrify it - feldspar or nepheline fills both roles.

Of course, this stoneware does not fire as white. But do you need white? Glazes will fire brightly colored on this surface. And, cleaner ball clays are available in many areas (even ball clays intended for casting will be plastic enough). It is also worth considering the use of a white engobe.

Feldspar/ball clay stoneware fits glazes, porcelain does not

Links

Glossary Stoneware
To potters, stonewares are simply high temperature, non-white bodies fired to sufficient density to make functional ware that is strong and durable.
Glossary Porcelaineous Stoneware
In ceramics, porcelains lack plasticity and fire to high density with white, glassy surface. Stonewares are plastic and fire cream to brown and lower density, Porcelaineous stoneware are between these two.
Articles Formulating a body using clays native to your area
Being able to mix your own clay body and glaze from native materials might seem ridiculous, yet Covid-19 taught us about the need for independence.
Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy