3899 | 3898 | 3897 | 3896 | 3890 | 3891 | 3892 | 3888 | 3889 | 3883 | 3885 | 3882 | 3880 | 3881 | 3878 | 3877 | 3876 | 3871 | 3872 | 3874 | 3869 | 3870 | 3866 | 3867 | 3864 | 3863 | 3862 | 3861 | 3860 | 3859 | 3838 | 3857 | 3858 | 3855 | 3856 | 3851 | 3853 | 3854 | 3849 | 3850 | 3852 | 3846 | 3848 | 3843 | 3840 | 3841 | 3842 | 3837 | 3836 | 3833 | 3831 | 3832 | 3829 | 3827 | 3828 | 3826 | 3824 | 3823 | 3822 | 3820 | 3819 | 3818 | 3815 | 3816 | 3817 | 3814 | 3813 | 3811 | 3810 | 3806 | 3807 | 3808 | 3805 | 3803 | 3802 | 3801 | 3800 | 3797 | 3798 | 3796 | 3793 | 3794 | 3792 | 3789 | 3786 | 3784 | 3787 | 3781 | 3779 | 3775 | 3773 | 3774 | 3772 | 3767 | 3768 | 3769 | 3762 | 3760 | 3759 | 3755 | 3752 | 3753 | 3754 | 3750 | 3748 | 3749 | 3742 | 3743 | 3745 | 3746 | 3747 | 3740 | 3737 | 3738 | 3739 | 3736 | 3734 | 3733 | 3732 | 3731 | 3729 | 3728 | 3726 | 3725 | 3724 | 3723 | 3721 | 3719 | 3720 | 3718 | 3716 | 3713 | 3712 | 3711 | 3710 | 3709 | 3707 | 3708 | 3706 | 3705 | 3704 | 3702 | 3701 | 3700 | 3699 | 3698 | 3695 | 3696 | 3697 | 3692 | 3693 | 3694 | 3690 | 3691 | 3689 | 3688 | 3685 | 3686 | 3679 | 3678 | 3676 | 3675 | 3674 | 3672 | 3673 | 3663 | 3664 | 3661 | 3656 | 3657 | 3658 | 3659 | 3651 | 3652 | 3654 | 3655 | 3650 | 3649 | 3648 | 3646 | 3647 | 3644 | 3645 | 3643 | 3642 | 3640 | 3639 | 3637 | 3636 | 3634 | 3635 | 3632 | 3631 | 3629 | 3630 | 3626 | 3627 | 3624 | 3625 | 3622 | 3623 | 3620 | 3619 | 3612 | 3610 | 3611 | 3606 | 3607 | 3608 | 3609 | 3602 | 3603 | 3604 | 3605 | 3601 | 3600 | 3599 | 3598 | 3596 | 3595 | 3594 | 3593 | 3591 | 3592 | 3588 | 3589 | 3585 | 3586 | 3584 | 3580 | 3581 | 3582 | 3583 | 3579 | 3577 | 3578 | 3576 | 3574 | 3572 | 3573 | 3571 | 3570 | 3568 | 3567 | 3565 | 3562 | 3563 | 3560 | 3561 | 3559 | 3557 | 3556 | 3555 | 3554 | 3553 | 3551 | 3552 | 3550 | 3549 | 3548 | 3547 | 3546 | 3544 | 3545 | 3543 | 3542 | 3538 | 3539 | 3540 | 3541 | 3536 | 3537 | 3535 | 3534 | 3531 | 3532 | 3533 | 3529 | 3530 | 3527 | 3528 | 3526 | 3525 | 3524 | 3523 | 3522 | 3520 | 3518 | 3516 | 3517 | 3515 | 3514 | 3512 | 3513 | 3511 | 3510 | 3509 | 3508 | 3507 | 3506 | 3505 | 3504 | 3046 | 3503 | 3493 | 3494 | 3490 | 3491 | 3486 | 3489 | 3485 | 3481 | 3483 | 3492 | 3479 | 3480 | 3476 | 3477 | 3474 | 3473 | 3471 | 3470 | 3469 | 3468 | 3465 | 3466 | 3467 | 3463 | 3459 | 3460 | 3461 | 3462 | 3458 | 3457 | 3456 | 3455 | 3454 | 3452 | 3449 | 3448 | 3447 | 3446 | 3445 | 3443 | 3444 | 3442 | 3441 | 3439 | 3440 | 3437 | 3438 | 3435 | 3436 | 3431 | 3433 | 3434 | 3430 | 3427 | 3428 | 3425 | 3426 | 3423 | 3422 | 3419 | 3421 | 3418 | 3415 | 3416 | 3417 | 3414 | 3413 | 3411 | 3412 | 3409 | 3410 | 3408 | 3401 | 3402 | 3403 | 3404 | 3406 | 3407 | 3400 | 3399 | 3397 | 3393 | 3394 | 3396 | 3392 | 3391 | 3387 | 3389 | 3390 | 3385 | 3384 | 3383 | 3382 | 3379 | 3380 | 3381 | 3378 | 3376 | 3375 | 3374 | 3373 | 3372 | 3370 | 3367 | 3368 | 3369 | 3364 | 3363 | 3360 | 3359 | 3358 | 3356 | 3355 | 3354 | 3352 | 3349 | 3348 | 3347 | 3344 | 3345 | 3346 | 3343 | 3342 | 3340 | 3338 | 3339 | 3337 | 3335 | 3336 | 3334 | 3333 | 3330 | 3322 | 3319 | 3320 | 3321 | 3317 | 3316 | 3313 | 3314 | 3315 | 3312 | 3310 | 3311 | 3309 | 3307 | 3308 | 3306 | 3304 | 3303 | 3302 | 3300 | 3301 | 3298 | 3299 | 3296 | 3295 | 3293 | 3294 | 3292 | 3291 | 3290 | 3289 | 3288 | 3286 | 3285 | 3284 | 3280 | 3281 | 3282 | 3278 | 3277 | 3272 | 3273 | 3274 | 3275 | 3276 | 3271 | 3270 | 3267 | 3268 | 3265 | 3266 | 3264 | 3262 | 3261 | 3260 | 3259 | 3258 | 3257 | 3256 | 3255 | 3253 | 3254 | 3251 | 3248 | 3247 | 3245 | 3246 | 3244 | 3241 | 3239 | 3236 | 3237 | 3235 | 3234 | 3233 | 3231 | 3232 | 3230 | 3229 | 3201 | 3202 | 3203 | 3204 | 3205 | 3206 | 3207 | 3208 | 3209 | 3210 | 3211 | 3212 | 3213 | 3214 | 3215 | 3216 | 3217 | 3219 | 3220 | 3222 | 3223 | 3224 | 3226 | 3227 | 3228 | 3199 | 3198 | 3197 | 3195 | 3196 | 3191 | 3192 | 3193 | 3194 | 3188 | 3189 | 3187 | 3185 | 3186 | 3183 | 3181 | 3182 | 3179 | 3180 | 3177 | 3176 | 3175 | 3174 | 3173 | 3169 | 3167 | 3164 | 3162 | 3159 | 3158 | 3157 | 3154 | 3155 | 3156 | 3153 | 3149 | 3150 | 3144 | 3145 | 3146 | 3147 | 3148 | 3142 | 3143 | 3139 | 3141 | 3138 | 3136 | 3137 | 3132 | 3135 | 3131 | 3130 | 3127 | 3124 | 3125 | 3126 | 3122 | 3123 | 3121 | 3120 | 3117 | 3119 | 3116 | 3112 | 3113 | 3114 | 3109 | 3110 | 3111 | 3098 | 3099 | 3102 | 3103 | 3104 | 3105 | 3106 | 3107 | 3108 | 3096 | 3094 | 3095 | 3091 | 3092 | 3093 | 3089 | 3090 | 3087 | 3086 | 3082 | 3083 | 3084 | 3080 | 3081 | 3079 | 3078 | 3077 | 3074 | 3075 | 3076 | 3073 | 3072 | 3070 | 3053 | 3055 | 3056 | 3057 | 3058 | 3059 | 3060 | 3061 | 3062 | 3063 | 3064 | 3065 | 3066 | 3067 | 3068 | 3069 | 3052 | 3050 | 3051 | 3048 | 3049 | 3047 | 3044 | 3043 | 3042 | 3041 | 3040 | 3038 | 3039 | 3037 | 3036 | 3035 | 3034 | 3033 | 3029 | 3030 | 3031 | 3023 | 3024 | 3021 | 3022 | 3019 | 3016 | 3017 | 3018 | 3015 | 3012 | 3013 | 3014 | 3011 | 3010 | 3007 | 3008 | 3009 | 3005 | 3006 | 3004 | 3001 | 3002 | 3003 | 2999 | 2995 | 2996 | 2994 | 2991 | 2992 | 2993 | 2990 | 2989 | 2986 | 2987 | 2988 | 2982 | 2983 | 2984 | 2985 | 2979 | 2980 | 2976 | 2977 | 2974 | 2973 | 2970 | 2971 | 2967 | 2968 | 2969 | 2966 | 2964 | 2965 | 2963 | 2961 | 2962 | 2960 | 2958 | 2952 | 2953 | 2954 | 2955 | 2956 | 2950 | 2951 | 2948 | 2949 | 2945 | 2946 | 2947 | 2944 | 2943 | 2939 | 2940 | 2941 | 2942 | 2937 | 2938 | 2936 | 2935 | 2929 | 2930 | 2931 | 2932 | 2933 | 2934 | 2928 | 2927 | 2925 | 2926 | 2921 | 2922 | 2923 | 2924 | 2919 | 2920 | 2917 | 2918 | 2915 | 2916 | 2913 | 2914 | 2912 | 2911 | 2910 | 2909 | 2907 | 2908 | 2906 | 2905 | 2903 | 2904 | 2900 | 2899 | 2898 | 2893 | 2894 | 2895 | 2896 | 2897 | 2890 | 2891 | 2892 | 2887 | 2888 | 2889 | 2885 | 2882 | 2883 | 2884 | 2880 | 2881 | 2878 | 2877 | 2872 | 2873 | 2874 | 2875 | 2876 | 2871 | 2868 | 2869 | 2870 | 2866 | 2867 | 2865 | 2864 | 2862 | 2863 | 2861 | 2860 | 2858 | 2859 | 2856 | 2857 | 2854 | 2855 | 2853 | 2852 | 2848 | 2849 | 2850 | 2847 | 2845 | 2846 | 2843 | 2842 | 2840 | 2841 | 2839 | 2838 | 2837 | 2836 | 2835 | 2833 | 2834 | 2832 | 2831 | 2828 | 2829 | 2827 | 2826 | 2825 | 2824 | 2822 | 2823 | 2820 | 2821 | 2819 | 2816 | 2815 | 2814 | 2813 | 2812 | 2811 | 2793 | 2794 | 2795 | 2796 | 2797 | 2798 | 2799 | 2800 | 2801 | 2802 | 2803 | 2804 | 2805 | 2806 | 2807 | 2808 | 2809 | 2810 | 2791 | 2792 | 2790 | 2787 | 2788 | 2784 | 2785 | 2786 | 2781 | 2782 | 2780 | 2777 | 2778 | 2779 | 2776 | 2775 | 2774 | 2772 | 2771 | 2769 | 2770 | 2768 | 2767 | 2766 | 2764 | 2765 | 2762 | 2763 | 2761 | 2760 | 2759 | 2758 | 2756 | 2752 | 2753 | 2754 | 2755 | 2750 | 2751 | 2748 | 2749 | 2747 | 2745 | 2746 | 2742 | 2743 | 2740 | 2741 | 2739 | 2737 | 2738 | 2736 | 2735 | 2734 | 2733 | 2732 | 2729 | 2730 | 2731 | 2728 | 2727 | 2726 | 2723 | 2724 | 2725 | 2722 | 2719 | 2720 | 2721 | 2718 | 2716 | 2715 | 2714 | 2713 | 2712 | 2711 | 2709 | 2708 | 2706 | 2707 | 2704 | 2705 | 2703 | 2702 | 2700 | 2693 | 2694 | 2695 | 2696 | 2697 | 2698 | 2699 | 2692 | 2690 | 2691 | 2689 | 2688 | 2687 | 2686 | 2685 | 2684 | 2683 | 2680 | 2681 | 2682 | 2678 | 2679 | 2677 | 2676 | 2675 | 2674 | 2673 | 2672 | 2671 | 2670 | 2669 | 2666 | 2668 | 2664 | 2665 | 2662 | 2663 | 2660 | 2661 | 2656 | 2657 | 2658 | 2659 | 2655 | 2654 | 2653 | 2652 | 2649 | 2650 | 2651 | 2646 | 2647 | 2648 | 2643 | 2644 | 2641 | 2642 | 2639 | 2640 | 2637 | 2638 | 2635 | 2636 | 2633 | 2634 | 2631 | 2632 | 2630 | 2629 | 2627 | 2628 | 2624 | 2626 | 2621 | 2622 | 2623 | 2618 | 2619 | 2617 | 2614 | 2615 | 2616 | 2613 | 2612 | 2607 | 2608 | 2609 | 2611 | 2606 | 2605 | 2602 | 2603 | 2604 | 2600 | 2601 | 2599 | 2598 | 2597 | 2595 | 2596 | 2591 | 2592 | 2593 | 2594 | 2585 | 2586 | 2587 | 2588 | 2589 | 2590 | 2584 | 2583 | 2582 | 2581 | 2578 | 2580 | 2576 | 2577 | 2573 | 2574 | 2575 | 2572 | 2571 | 2566 | 2567 | 2569 | 2570 | 2563 | 2565 | 2562 | 2561 | 2560 | 2558 | 2559 | 2557 | 2556 | 2554 | 2555 | 2551 | 2552 | 2548 | 2549 | 2550 | 2547 | 2545 | 2546 | 2542 | 2543 | 2544 | 2540 | 2541 | 2539 | 2537 | 2536 | 2533 | 2534 | 2535 | 2531 | 2532 | 2530 | 2528 | 2525 | 2526 | 2527 | 2522 | 2523 | 2521 | 2519 | 2520 | 2518 | 2517 | 2516 | 2515 | 2514 | 2513 | 2511 | 2512 | 2509 | 2510 | 2508 | 2506 | 2507 | 2505 | 2504 | 2503 | 2502 | 2501 | 2499 | 2490 | 2494 | 2495 | 2496 | 2497 | 2498 | 2489 | 2488 | 2487 | 2486 | 2485 | 2484 | 2483 | 2482 | 2481 | 2479 | 2480 | 2478 | 2474 | 2475 | 2476 | 2477 | 2472 | 2473 | 2471 | 2470 | 2465 | 2466 | 2467 | 2468 | 2469 | 2464 | 2461 | 2460 | 2459 | 2458 | 2457 | 2454 | 2455 | 2456 | 2451 | 2452 | 2453 | 2449 | 2450 | 2447 | 2448 | 2442 | 2443 | 2444 | 2445 | 2446 | 2440 | 2441 | 2439 | 2436 | 2437 | 2438 | 2434 | 2435 | 2433 | 2432 | 2429 | 2430 | 2431 | 2425 | 2426 | 2427 | 2428 | 2422 | 2423 | 2424 | 2421 | 2417 | 2418 | 2419 | 2420 | 2416 | 2415 | 2412 | 2411 | 2410 | 2408 | 2409 | 2407 | 2406 | 2405 | 2403 | 2404 | 2402 | 2401 | 2400 | 2399 | 2398 | 2397 | 2396 | 2395 | 2394 | 2392 | 2393 | 2390 | 2389 | 2387 | 2386 | 2385 | 2384 | 2383 | 2380 | 2375 | 2376 | 2377 | 2378 | 2379 | 2374 | 2373 | 2372 | 2371 | 2369 | 2370 | 2366 | 2368 | 2361 | 2362 | 2363 | 2364 | 2365 | 2360 | 2359 | 2355 | 2356 | 2357 | 2354 | 2353 | 2350 | 2351 | 2348 | 2349 | 2346 | 2347 | 2344 | 2345 | 2343 | 2342 | 2341 | 2337 | 2339 | 2340 | 2335 | 2336 | 2334 | 2333 | 2328 | 2329 | 2330 | 2331 | 2332 | 2327 | 2326 | 2323 | 2324 | 2325 | 2322 | 2321 | 2316 | 2317 | 2318 | 2319 | 2320 | 2314 | 2315 | 2311 | 2312 | 2313 | 2309 | 2308 | 2306 | 2307 | 2304 | 2305 | 2303 | 2299 | 2300 | 2301 | 2297 | 2294 | 2295 | 2296 | 2292 | 2278 | 2279 | 2280 | 2282 | 2283 | 2284 | 2285 | 2286 | 2287 | 2288 | 2289 | 2290 | 2273 | 2274 | 2275 | 2276 | 2277 | 2271 | 2270 | 2269 | 2266 | 2265 | 2263 | 2264 | 2262 | 2260 | 2261 | 2259 | 2258 | 2257 | 2255 | 2256 | 2254 | 2250 | 2252 | 2249 | 2247 | 2248 | 2246 | 2242 | 2243 | 2245 | 2239 | 2240 | 2241 | 2235 | 2236 | 2237 | 2238 | 2234 | 2233 | 2232 | 2231 | 2230 | 2229 | 2225 | 2226 | 2224 | 2222 | 2223 | 2220 | 2221 | 2218 | 2219 | 2216 | 2217 | 2214 | 2215 | 2213 | 2211 | 2212 | 2210 | 2209 | 2208 | 2207 | 2206 | 2205 | 2203 | 2204 | 2202 | 2201 | 2199 | 2200 | 2198 | 2197 | 2195 | 2196 | 2194 | 2192 | 2193 | 2191 | 2189 | 2190 | 2188 | 2186 | 2187 | 2185 | 2184 | 2182 | 2183 | 2180 | 2178 | 2179 | 2176 | 2177 | 2172 | 2173 | 2174 | 2175 | 2171 | 2166 | 2167 | 2169 | 2170 | 2165 | 2156 | 2157 | 2158 | 2159 | 2161 | 2162 | 2164 | 2153 | 2154 | 2155 | 2151 | 2150 | 2148 | 2149 | 2142 | 2143 | 2144 | 2145 | 2146 | 2147 | 2140 | 2141 | 2138 | 2139 | 2136 | 2137 | 2135 | 2129 | 2130 | 2131 | 2132 | 2133 | 2134 | 2128 | 2127 | 2126 | 2125 | 2124 | 2121 | 2122 | 2123 | 2118 | 2117 | 2115 | 2116 | 2114 | 2113 | 2112 | 2111 | 2109 | 2108 | 2107 | 2106 | 2104 | 2105 | 2101 | 2102 | 2103 | 2099 | 2100 | 2096 | 2094 | 2095 | 2093 | 2092 | 2091 | 2089 | 2090 | 2088 | 2087 | 2086 | 2085 | 2084 | 2082 | 2083 | 2081 | 2078 | 2079 | 2080 | 2076 | 2077 | 2073 | 2074 | 2075 | 2071 | 2069 | 2066 | 2067 | 2068 | 2064 | 2060 | 2061 | 2062 | 2059 | 2057 | 2058 | 2052 | 2053 | 2054 | 2055 | 2056 | 2049 | 2050 | 2051 | 2048 | 2047 | 2046 | 2042 | 2043 | 2044 | 2045 | 2040 | 2039 | 2038 | 2036 | 2035 | 2029 | 2030 | 2031 | 2033 | 2034 | 2027 | 2024 | 2025 | 2026 | 2017 | 2018 | 2019 | 2020 | 2021 | 2022 | 2016 | 2015 | 2014 | 2013 | 2010 | 2011 | 2012 | 2008 | 2009 | 2007 | 2001 | 2002 | 2003 | 2004 | 2005 | 1993 | 1995 | 1998 | 2000 | 1990 | 1991 | 1987 | 1988 | 1986 | 1983 | 1984 | 1976 | 1977 | 1978 | 1979 | 1980 | 1981 | 1974 | 1975 | 1973 | 1972 | 1970 | 1968 | 1969 | 1967 | 1966 | 1965 | 1964 | 1962 | 1961 | 1959 | 1960 | 1955 | 1956 | 1957 | 1954 | 1952 | 1953 | 1950 | 1951 | 1948 | 1947 | 1946 | 1944 | 1945 | 1940 | 1941 | 1942 | 1943 | 1939 | 1934 | 1935 | 1936 | 1937 | 1938 | 1932 | 1933 | 1931 | 1930 | 1928 | 1927 | 1922 | 1923 | 1924 | 1925 | 1926 | 1916 | 1918 | 1919 | 1920 | 1921 | 1915 | 1914 | 1906 | 1907 | 1908 | 1909 | 1910 | 1911 | 1912 | 1913 | 1902 | 1904 | 1905 | 1895 | 1896 | 1897 | 1899 | 1900 | 1901 | 1891 | 1893 | 1894 | 1890 | 1888 | 1889 | 1887 | 1885 | 1882 | 1883 | 1884 | 1874 | 1875 | 1876 | 1877 | 1878 | 1879 | 1870 | 1871 | 1872 | 1873 | 1868 | 1867 | 1866 | 1865 | 1864 | 1858 | 1859 | 1860 | 1861 | 1862 | 1863 | 1854 | 1855 | 1850 | 1851 | 1852 | 1848 | 1849 | 1846 | 1847 | 1843 | 1844 | 1845 | 1842 | 1831 | 1832 | 1833 | 1834 | 1835 | 1836 | 1838 | 1839 | 1840 | 1841 | 1828 | 1829 | 1830 | 1827 | 1826 | 1825 | 1823 | 1824 | 1818 | 1819 | 1820 | 1821 | 1822 | 1817 | 1815 | 1816 | 1814 | 1812 | 1811 | 1809 | 1810 | 1807 | 1806 | 1805 | 1804 | 1803 | 1802 | 1796 | 1797 | 1798 | 1799 | 1800 | 1801 | 1792 | 1793 | 1794 | 1791 | 1790 | 1789 | 1788 | 1786 | 1785 | 1781 | 1782 | 1783 | 1784 | 1780 | 1779 | 1776 | 1775 | 1772 | 1773 | 1770 | 1769 | 1768 | 1767 | 1763 | 1765 | 1766 | 1762 | 1760 | 1761 | 1757 | 1758 | 1759 | 1755 | 1749 | 1750 | 1751 | 1752 | 1753 | 1754 | 1748 | 1747 | 1745 | 1744 | 1742 | 1743 | 1740 | 1736 | 1737 | 1735 | 1733 | 1732 | 1729 | 1722 | 1723 | 1716 | 1717 | 1718 | 1715 | 1714 | 1712 | 1713 | 1711 | 1710 | 1709 | 1708 | 1706 | 1705 | 1699 | 1700 | 1701 | 1702 | 1703 | 1704 | 1693 | 1694 | 1695 | 1696 | 1697 | 1692 | 1687 | 1690 | 1691 | 1685 | 1686 | 1683 | 1684 | 1682 | 1681 | 1679 | 1677 | 1678 | 1675 | 1674 | 1671 | 1672 | 1669 | 1668 | 1665 | 1666 | 1667 | 1663 | 1662 | 1659 | 1658 | 1657 | 1654 | 1655 | 1656 | 1650 | 1647 | 1648 | 1649 | 1638 | 1637 | 1636 | 1635 | 1628 | 1623 | 1625 | 1626 | 1627 | 1618 | 1619 | 1622 | 1614 | 1615 | 1616 | 1617 | 1613 | 1603 | 1606 | 1607 | 1608 | 1609 | 1611 | 1612 | 1591 | 1592 | 1593 | 1594 | 1595 | 1596 | 1597 | 1598 | 1599 | 1600 | 1602 | 1578 | 1579 | 1580 | 1581 | 1582 | 1583 | 1584 | 1585 | 1586 | 1587 | 1588 | 1589 | 1590 | 1576 | 1577 | 1575 | 1574 | 1573 | 1288 | 1570 | 1565 | 1566 | 1567 | 1568 | 1564 | 1560 | 1559 | 1555 | 1556 | 1557 | 1558 | 1551 | 1553 | 1554 | 1548 | 1549 | 1550 | 1547 | 1545 | 1546 | 1543 | 1544 | 1537 | 1538 | 1542 | 1533 | 1531 | 1529 | 1528 | 1525 | 1526 | 1527 | 1523 | 1524 | 1521 | 1520 | 1517 | 1518 | 1519 | 1515 | 1516 | 1509 | 1510 | 1511 | 1504 | 1505 | 1506 | 1507 | 1508 | 1499 | 1500 | 1501 | 1502 | 1503 | 1497 | 1498 | 1493 | 1494 | 1495 | 1496 | 1489 | 1488 | 1487 | 1485 | 1484 | 1479 | 1481 | 1483 | 1621 | 1477 | 1476 | 1472 | 1473 | 1471 | 1470 | 1468 | 1469 | 1467 | 1454 | 1457 | 1458 | 1459 | 1460 | 1461 | 1462 | 1463 | 1452 | 1451 | 1446 | 1447 | 1448 | 1449 | 1450 | 1442 | 1443 | 1432 | 1435 | 1436 | 1437 | 1439 | 1396 | 1399 | 1401 | 1402 | 1403 | 1404 | 1405 | 1407 | 1408 | 1409 | 1410 | 1411 | 1412 | 1413 | 1414 | 1418 | 1419 | 1420 | 1421 | 1422 | 1423 | 1424 | 1425 | 1426 | 1427 | 1429 | 1430 | 1341 | 1342 | 1343 | 1344 | 1391 | 1392 | 1393 | 1394 | 1339 | 1340 | 1337 | 1329 | 1330 | 1331 | 1332 | 1333 | 1335 | 1328 | 1327 | 1321 | 1322 | 1323 | 1324 | 1325 | 1320 | 1301 | 1302 | 1303 | 1304 | 1305 | 1306 | 1307 | 1308 | 1309 | 1310 | 1311 | 1312 | 1313 | 1314 | 1315 | 1297 | 1298 | 1299 | 1300 | 1291 | 1292 | 1293 | 1295 | 1296 | 1290 | 1280 | 1281 | 1282 | 1285 | 1286 | 1287 | 1279 | 1276 | 1277 | 1278 | 1275 | 1264 | 1265 | 1266 | 1268 | 1269 | 1270 | 1271 | 1272 | 1273 | 1261 | 1262 | 1259 | 1260 | 1257 | 1258 | 1255 | 1254 | 1252 | 1250 | 1249 | 1247 | 1243 | 1244 | 1245 | 1246 | 1241 | 1242 | 1240 | 1238 | 1239 | 1237 | 1236 | 1235 | 1231 | 1232 | 1233 | 1234 | 1228 | 1229 | 1230 | 1224 | 1225 | 1226 | 1223 | 1220 | 1221 | 1222 | 1215 | 1216 | 1217 | 1218 | 1211 | 1212 | 1213 | 1214 | 1209 | 1210 | 1208 | 1202 | 1204 | 1205 | 1206 | 1200 | 1201 | 1199 | 1196 | 1198 | 1192 | 1193 | 1189 | 1190 | 1191 | 1185 | 1178 | 1179 | 1182 | 1184 | 1166 | 1167 | 1168 | 1169 | 1171 | 1173 | 1174 | 1164 | 1163 | 1153 | 1154 | 1155 | 1156 | 1157 | 1158 | 1159 | 1160 | 1161 | 1151 | 1152 | 1147 | 1148 | 1149 | 1146 | 1142 | 1143 | 1144 | 1145 | 1138 | 1139 | 1140 | 1136 | 1133 | 1134 | 1135 | 1132 | 629 | 1130 | 1131 | 1129 | 1123 | 1124 | 1125 | 1126 | 1127 | 1128 | 1122 | 1121 | 1120 | 1119 | 1116 | 1117 | 1118 | 1115 | 1114 | 1109 | 1111 | 1112 | 1113 | 1107 | 1106 | 1099 | 1100 | 1101 | 1102 | 1103 | 1098 | 1094 | 1095 | 1097 | 1093 | 1091 | 1092 | 1089 | 1090 | 1088 | 1085 | 1086 | 1081 | 1082 | 1078 | 1079 | 1080 | 1076 | 1077 | 1075 | 1074 | 743 | 1072 | 1073 | 1070 | 1071 | 1069 | 1068 | 1067 | 1057 | 1058 | 1059 | 1060 | 1061 | 1062 | 1063 | 1064 | 1065 | 1066 | 1055 | 730 | 1047 | 1048 | 1049 | 1050 | 1051 | 1052 | 1053 | 1042 | 1043 | 1044 | 1045 | 1046 | 1036 | 1037 | 1038 | 1039 | 1040 | 1041 | 1034 | 1035 | 910 | 1032 | 935 | 1030 | 1031 | 1026 | 1027 | 1028 | 1029 | 1024 | 1025 | 1023 | 1021 | 1022 | 1018 | 1019 | 1020 | 1017 | 684 | 1016 | 1015 | 890 | 1014 | 1011 | 1012 | 1013 | 1010 | 1009 | 1008 | 1007 | 660 | 1006 | 690 | 1005 | 1002 | 1003 | 997 | 999 | 1000 | 1001 | 996 | 995 | 994 | 987 | 988 | 989 | 990 | 991 | 992 | 984 | 985 | 986 | 431 | 983 | 982 | 979 | 980 | 981 | 961 | 977 | 978 | 975 | 976 | 972 | 974 | 969 | 970 | 971 | 968 | 911 | 967 | 817 | 850 | 853 | 658 | 659 | 439 | 966 | 964 | 962 | 963 | 960 | 958 | 959 | 957 | 954 | 955 | 956 | 952 | 953 | 949 | 950 | 951 | 947 | 948 | 946 | 945 | 944 | 943 | 942 | 941 | 938 | 936 | 937 | 934 | 931 | 932 | 933 | 752 | 292 | 815 | 816 | 819 | 316 | 832 | 839 | 846 | 847 | 854 | 855 | 863 | 864 | 865 | 362 | 879 | 888 | 891 | 918 | 689 | 716 | 722 | 724 | 741 | 744 | 746 | 749 | 750 | 929 | 927 | 928 | 925 | 926 | 924 | 153 | 923 | 919 | 920 | 921 | 916 | 914 | 912 | 908 | 909 | 905 | 906 | 464 | 354 | 904 | 878 | 900 | 893 | 894 | 895 | 896 | 897 | 892 | 898 | 899 | 889 | 351 | 885 | 886 | 880 | 881 | 883 | 884 | 667 | 874 | 875 | 361 | 930 | 940 | 430 | 434 | 873 | 825 | 826 | 828 | 829 | 844 | 845 | 849 | 852 | 856 | 857 | 858 | | 860 | 870 | 697 | 764 | 862 | 861 | 818 | 851 | 663 | 830 | 831 | 833 | 834 | 835 | 836 | 838 | 840 | 842 | 843 | 824 | 837 | 822 | 820 | 801 | 810 | 811 | 812 | 814 | 628 | 656 | 657 | 661 | 664 | 665 | 666 | 668 | 669 | 670 | 674 | 675 | 677 | 678 | 680 | 681 | 682 | 683 | 685 | 686 | 687 | 688 | 691 | 692 | 693 | 694 | 696 | 698 | 699 | 700 | 701 | 702 | 703 | 704 | 705 | 713 | 459 | 717 | 719 | 720 | 721 | 725 | 729 | 731 | 734 | 736 | 737 | 740 | 748 | 751 | 754 | 755 | 756 | 757 | 758 | 759 | 760 | 761 | 762 | 711 | 813 | 809 | 808 | 803 | 804 | 805 | 364 | 802 | 800 | 798 | 796 | 797 | 795 | 791 | 792 | 793 | 794 | 461 | 790 | 787 | 788 | 770 | 771 | 772 | 773 | 774 | 775 | 777 | 782 | 784 | 768 | 769 | 767 | 765 | 766 | 626 | 726 | 727 | 728 | 710 | 706 | 295 | 444 | 484 | 652 | 654 | 655 | 643 | 646 | 647 | 648 | 649 | 650 | 630 | 631 | 633 | 634 | 635 | 638 | 639 | 640 | 564 | 578 | 579 | 582 | 583 | 584 | 587 | 588 | 590 | 591 | 592 | 593 | 594 | 595 | 596 | 597 | 598 | 599 | 600 | 601 | 602 | 603 | 604 | 605 | 606 | 607 | 608 | 609 | 610 | 611 | 613 | 614 | 615 | 616 | 617 | 618 | 619 | 620 | 623 | 438 | 442 | 443 | 447 | 448 | 455 | 465 | 466 | 472 | 473 | 481 | 482 | 483 | 576 | 575 | 562 | 532 | 535 | 537 | 539 | 541 | 543 | 545 | 547 | 551 | 553 | 555 | 513 | 514 | 515 | 516 | 517 | 518 | 519 | 520 | 521 | 522 | 523 | 524 | 525 | 526 | 527 | 528 | 530 | 500 | 501 | 502 | 503 | 504 | 505 | 506 | 507 | 508 | 509 | 511 | 487 | 488 | 489 | 491 | 492 | 495 | 496 | 499 | 458 | 456 | 360 | 294 | 293 | 415 | 416 | 404 | 402 | 398 | 401 | 377 | 386 | 372 | 369 | 368 | 358 | 344 | 353 | 355 | 321 | 322 | 325 | 319 | 257 | 8 | 13 | 14 | 271 | 272 | 33 | 289 | 34 | 35 | 296 | 44 | 45 | 86 | 98 | 100 | 106 | 117 | 139 | 145 | 159 | 182 | 183 | 184 | 185 | 210 | 211 | 212 | 216 | 222 | 223 | 235 | 239 | 240 | 243 | 246 | 248 | 250 | 3587 | 3590 | 3160

The unexpected reason for this crazing can be seen in the chemistry

The glaze is 10% calcium carbonate added to Ravenscrag slip. Ravenscrag Slip does not craze when used by itself as a glaze at cone 10R on this body, so why would adding a relatively low expansion flux like CaO make it craze? This is an excellent example of the value of looking at the chemistry (the three are shown side-by-side in my account at Insight-live.com). The added CaO pushes the very-low-expansion Al2O3 and SiO2 down by 30% (in the unity formula), so the much higher expansion of all the others drives the COE of the whole way up. And talc? It contains SiO2 (so the SiO2 is not driven down nearly as much) and its MgO has a much lower expansion than CaO does.

Glaze chemistry explains the crazing

Related Pictures

You cannot fix this crazing with a process or firing change


This picture has its own page with more detail, click here to see it.

This is severe crazing (at cone 10R). It is happening because of the chemistry of the glaze, not the firing. The first option to check when fixing crazing is: Can the glaze accept an addition of SiO2? This glaze is an excellent candidate for that because the melt is highly fluid, it will surely be able to dissolve extra SiO2. But it could also accept Al2O3 because it is highly glossy (a little extra Al2O3 will not matte it and would also reduce expansion and increase fired hardness and durability). What to do then? I would start with a 10% addition of a mix of two parts silica to one part kaolin (this mix has a 10:1 SiO2:Al2O3 ratio, about the same as most glossy glazes).

CaO is a strong flux but it can cause crazing


This picture has its own page with more detail, click here to see it.

2, 5, 10, 15% calcium carbonate added to Ravenscrag Slip on a buff stoneware fired at cone 10R. It gets progressively glossier toward 15%, crazing starts at 10% (test by Kat Valenzuela). Adding a flux only reduces the SiO2 and Al2O3, this pushes the thermal expansion upwards. 5% is actually sufficient. An alternative would be to use wollastonite, it supplies SiO2 also.

GR10-B Ravenscrag transparent glaze (with 10 talc)


This picture has its own page with more detail, click here to see it.

Because this glaze employs 10% dolomite instead of 10% calcium carbonate it has a lower thermal expansion and is less likely to craze. While the dolomite is contributing MgO, which normally mattes glazes, there is not enough to do it here.

Links

Materials Talc
A source of MgO for ceramic glazes, a flux or thermal expansion additive in clay bodies, also used in the manufacture of cordierite.
Glossary Calculated Thermal Expansion
Calculation of the thermal expansion of glazes is a very useful comparative glaze-fit tool. But it’s not a laboratory measurement.
Glossary Glaze Chemistry
Glaze chemistry is the study of how the oxide chemistry of glazes relate to the way they fire. It accounts for color, surface, hardness, texture, melting temperature, thermal expansion, etc.
Troubles Glaze Crazing
Ask the right questions to analyse the real cause of glaze crazing. Do not just treat the symptoms, the real cause is thermal expansion mismatch with the body.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy