This is G1214Z1 brushing glaze (with 5% titanium added). For a 340g powder batch (to get a pint) my initial target is 5g CMC gum and 5g Veegum. CMC controls drying speed and Veegum the amount of gelling. I first mix the CMC with the powder and shake the whole batch in a plastic bag. Then I add it all to 440g of water in the blender jar and mix it well (making sure no agglomerates remain (stage 1). Stage 2 is adding the VeeGum slowly, while high-speed blender-mixing, this is important because it enables tuning the degree of gel (which cannot be predicted). Because this recipe has little clay, it took all 5g of Veegum without overgelling (the entire mass moved freely in the mixer jar). But it did gel overnight (so 4g would be better next time). By contrast, it is the brushing behavior that demonstrates whether the amount of CMC is right. Not enough and coats dry too fast and go on too thick. Too much and it dries too slowly and too many coats are needed.

This picture has its own page with more detail, click here to see it.
The cone 6 mug on the left has the G3933A glaze, applied as a dipping glaze. It turned out poorly - crawling from corners and looking thin and washed out. I made a brushing glaze version of this (which adds 1.5% CMC gum), I keep it around for this very purpose. It has a high specific gravity (unlike commercial ones that have high water contents - they will run and go on too thin if you try this). Because of the gum, it dries hard, there is no shrinkage or cracking. On a second firing, using the C6DHSC schedule again, (mug on the right) the surface is transformed - thicker, more vibrant color.
It is possible to make a small brushing batch by simply dewatering some of the dipping glaze on a plaster bat (just for a minute or two, long enough to pull out the water). Then remix it with enough gum solution to get a paintable consistency. It doesn’t have to be precise, just get it to a point where it paints on and sticks in the thickness you need and does not crack on drying.

This picture has its own page with more detail, click here to see it.
This is CMC gum 35g/liter gum solution after it has been thoroughly hot-mixed and cooled to about 30C. As it cools further and sits it thins. Gum solutions can have a higher CMC content, up to double this, but they are more difficult to use.
Most often, gum solution is intended to augment the water when batching a recipe - not adding to a glaze slurry. This is because adding enough to have any effect on an already-mixed glaze thins it (so an equal amount or more water should first be removed). For example, consider converting a dipping glaze to a brushing glaze: Adding the equivalent of 1.5% CMC gum powder, via this gum solution, to a gallon of glaze would also add almost a liter of water. Better to blender mix in the CMC power. CMC gum is often used in consort with a gelling agent like VeeGum, enabling more water (this is done in many commercial bottled glazes).

This picture has its own page with more detail, click here to see it.
This is the most viscous suspension we can make using hot water and a propeller mixer - 300ml water with 13.25g Veegum CER. In glazes having low clay content adding this gels the slurry, enabling higher water content to improve its brushing properties and slow down drying. In slurries having plenty of clay pure CMC gum is usually better (unless a high-water-content slurry is needed). Of course, keep in mind that anything with CMC gum can be subject to microbial attack.

This picture has its own page with more detail, click here to see it.
In order to add 0.5% CMC gum to this already-mixed glaze I need to know how much powder is present. Here’s how:
Put a teaspoon of the slurry (well stirred) on the tared-tray of an accurate gram scale. In this case it weighed 5.04g. The tray was just dried under a heat lamp, the scale now reports 2.46g. The water content of the slurry is thus (5.04 - 2.46) / 5.04 * 100 = 51.2% (making the solids content 48.8%). The glaze slurry weighs 645g. 48.8% of that = 315g of powder. 0.5% of 315 = 1.6g of CMC gum to blender mix into this.

This picture has its own page with more detail, click here to see it.
Let's make a DIY low SG version of G2934BL. Weigh out 340g of dipping glaze powder. Include 5g Veegum (to gel the slurry to enable more than normal water) and 5g CMC gum (for slow drying and brushing properties). Shake-mix all the powder in a plastic bag. Pour it into 440g water, blender mix on low speed, then finish with 20 seconds on high speed. This fills a 500ml jar. In subsequent batches, I adjust the Veegum for more or less gel, the CMC for slower or faster drying and the water amount for thicker or thinner painted layers. Dipping glaze recipes can and do respond differently to the gums. Those having little clay content work well (e.g. reactive and crystalline glazes). If bentonite is present, it is often best to leave it out. Recipes having high percentages of ball clay or kaolin might work best with less Veegum. Keep good notes (with pictures) to reach the objective of good brushing properties. Use code-numbering on the jars and test pieces.
Here is some incentive: Brushing glazes have gotten to the point where it can cost $5 to glaze one mug! This is so worthwhile doing that I make custom labels for each jar!
| Glossary |
Brushing Glaze
Hobbyists and increasing numbers of potters use commercial paint-on glazes. It's convenient, there are lots of visual effects. There are also issues compared to dipping glazes. You can also make your own. |
| Glossary |
Rheology
In ceramics, this term refers to the flow and gel properties of a glaze or body suspension (made from water and mineral powders, with possible additives, deflocculants, modifiers). |
| Glossary |
Micro Organisms
Ceramic glazes and clay bodies can host micro organisms. They can be just a nuisance, a source of worry or can render a product useless. What should you do? |
| Materials |
CMC Gum
CMC gum is indispensable for many types of ceramic glazes. It is a glue and is mainly used to slow drying and improve adhesion and dry hardness. |
| Materials |
Veegum
A clay of incredibly small particle size. It has the highest plasticity of any known clay and acts as a suspending and gelling agent in slurries. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
Buy me a coffee and we can talk