Color like this, from commercial brushing glazes, has become so trendy that multiple problems associated with it are being ignored by potters and hobbyists at cone 6. First, crazing (this network of fine cracks): When people use dense-burning bodies, ware doesn't leak, so it is deemed to be OK. When ware is made using stoneware clays having higher porosities, and it leaks, the clay bodies are blamed. And the poor strength resulting from the crazing is also blamed on the clay. However, this potter has done two right things:
1. Using an iron-stained honey glaze on the inside (e.g. GA6-B). It does not, cannot, leach heavy metals. Many are misinterpreting the ASTM D-4236 label on glaze jars and using intense heavy metal colored glazes on food surfaces!
2. The honey glaze inside does not craze so the mug does not leak even though the body has a higher porosity than the supposed vitrification magic number of <0.5%.
The bottom line: Use glazes that don't craze, DIY ones if possible or necessary, don't use really bright colors on food surfaces.
I waited for a week for someone to notice this was AI-generated. I used an AI image because a real piece would offend the maker. AI produced this on first try as representative of what's on social. AI photos are less authentic than DIY, so are pieces made in isolation of awareness of the critical design and safety flaws outlined here. This page gives part of the solution and links to full solutions.
AI generated with a prompt for a mug with layered glazes, crazing and representative of what is on social. AI Policy
AI-generated using prompt for drippy and layer glazed pottery typically displayed on social. AI PolicyThis picture has its own page with more detail, click here to see it.
There is an undeniable appeal to the bright colors of many commercial glazes. While nobody is recommending abandoning them and going all-in on DIY, there is an appeal to having more control. If you are a potter, hobbyist or small manufacturer, consider: Do we want customers eating and drinking from these kinds of glazes? This type of ware is often crazed (runny glazes do that, especially on bodies they were not designed to fit). These are also prime candidates for leaching the high percentages of the heavy metals they contain. All those drippy layers running and pooling on the insides can make pieces into glaze compression time bombs. For food surfaces, the glaze manufacturers want us using their recommended balanced, lightly colored products. Good news! These base recipes are also the easiest to make yourself. When did we get intimidated about mixing our own glazes anyway? No one has to go full mad scientist on DIY here. Research the common ingredients your supplier offers. Use recipes that pass a sanity test. Be a savvy consumer - these colored products are expensive and using them only on the outsides will cut your costs in half. Learn to add pigments to your base recipes and save even more. Then learn to make and use dipping glazes (not dripping glazes) and save time also.
| Glossary |
Commercial hobby brushing glazes
These are an incredible benefit to pottery beginners and pure hobbyists. But they can also be an obstacle to progress and affordability as your skills improve. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
Buy me a coffee and we can talk