Fired at 350F/hr to 1700F and held for 15 minutes. 3110 is finally starting to move. 3134 also (being full of bubbles). Gerstley Borate has turned almost transparent (because the Colemanite portion of it is now melting). 3195 is looking very well behaved compared to most others, forming a bubble free glass of high surface tension (F15 and F524 are starting to do the same).
| Temperatures | Comparison of frit melts at 1700F (926-) |
| Materials |
Fusion Frit F-524
A low fire base glaze, add 10% kaolin, adjust thermal expansion using other frits. |
| Materials |
Fusion Frit FZ-16
The champion in our frit melt-off competitition. This frit showcases the amazing fluxing power of boron and zinc working together. It is 15.5% ZnO. |
| Materials |
Fusion Frit F-75
High sodium, high thermal expansion low boron frit. An equivalent of Ferro Frit 3110. |
| Materials |
Fusion Frit F-69
A magnesia borosilicate frit having very low thermal expansion and melting point. Commonly used as a substitute for Ferro frit 3249. |
| Materials |
Fusion Frit F-38
High strontium low alumina borosilicate flux. |
| Materials |
Fusion Frit F-15
|
| Materials |
Ferro Frit 3602
A lead bisilicate frit with 2.5% alumina oxide. |
| Materials |
Frit B325
|
| Materials |
Frit LA-300
|
| Materials |
Ferro Frit 3249
A magnesia borosilicate frit. Very low thermal expansion. Invaluable for increasing the MgO in glazes (to prevent crazing and create matteness). Low melting. |
| Materials |
Ferro Frit 3195
A commonly available calcium borosilicate frit. It is glaze-like, needing only a kaolin addition to create a low-temperature semi-glossy glaze. |
| Materials |
Ferro Frit 3134
A frit with 23% B2O3. The most common of frits used in pottery in North America. Around the world, other companies make frits of equivalent chemistry. |
| Materials |
Ferro Frit 3124
A commonly available calcium borosilicate frit. It is glaze-like, needing only a kaolin addition to create a low-temperature glossy glaze. |
| Materials |
Ferro Frit 3110
High sodium, high thermal expansion low boron frit. A super-feldspar in clay bodies. Melts at very low temperatures. Useful to make crackle glazes. |
| Projects | Comparing the Melt Fluidity of 16 Frits |