It is made from 85% Ferro Frit 3134, 7.5% kaolin and 7.5% silica. While not obvious from the recipe, one look at the chemistry of this (as displayed when you enter a recipe into your account at insight-live.com) will show very low Al2O3. Frit 3134 has almost no Al2O3, yet it is an essential component of functional glazes (for durability, resistance to crystallization, stability during firing). The kaolin is the only contributor of Al2O3 and there is only a little. A simple fix would be to use Ferro Frit 3124 instead, remove the silica and increase the kaolin to 15.
| Glossary |
Boron Blue
Boron blue is a glaze fault involving the crystallization of calcium borate. It can be solved using glaze chemistry. |