0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silica:Alumina Ratio | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Material Sense

Ceramic glaze and body recipes often need material substitution or just scrutiny. Their chemistry, mineralogy and physical properties all need consideration.

Key phrases linking here: material substitution, material sense - Learn more

Details

Material substitution in bodies, slips, engobes and glazes is a constant and ongoing part of most ceramic enterprises. Often, lack of availability, quality issues and price are motivating factors. "Materials sense" can also save much time and effort by enabling recipe logic. With these, potters and technicians can often identify problems with recipes simply by noting unusual combinations of materials, their percentages or whether they even belong in that type of recipe.

In Glazes, Undergazes

In ceramics, glazes fire the way they do primarily because of their chemistry. The most basic substitution is to simply replace one material for another of the same type (and thus a similar chemistry). This is often possible with different brand names of the same mineral or a refined generic material (e.g. calcium carbonate, zinc oxide, dolomite). The more complex the chemistry of the raw material, the more likely are issues with changes to another (e.g. feldspar, spodumene). In some cases, substitution recipes are recommended where a mix of two or more other materials is said to be an equivalent. In more complicated cases, the substitution involves substituting one material for another and removing a related amount of one or more others (e.g., substituting petalite to, or for, lithium carbonate). Another problem can occur where, although the chemistry of the substitute is very similar, it's physical properties or particle physics are different enough to affect the working properties of the glaze slurry (e.g. a kaolin). Frit substitutions can be more complex, especially when glaze chemistry is needed to supply the same mix of oxides from mixes of multiple frits and other materials. Metal oxide and stain substitutions can be even more difficult; the color shade can be a combination of percentage, the chemistry of the stain and the chemistry of the host glaze.

A given chemistry can be supplied by many different mixes of refined and raw material powders, each of these having advantages and disadvantages regarding price, ease of use in production, toxicity, etc. It is common to use glaze chemistry to calculate how to juggle a recipe to substitute one material for another of slightly or even very different chemistry while maintaining the chemistry of the glaze as a whole. The calculation is more complex when the substitute brings along other oxides not in the material being substituted (or fewer) or the original or substitute has a very different weight loss on firing (LOI). As noted, frits especially can have complex chemistries and obviously it is more complicated if they are involved in the substitution calculation.

In Bodies, Engobes, Slips

Materials are employed for their physical presence (e.g. plasticity) and firing characteristics (not for chemistry). Thus, testing must be done to see how maturity, drying properties, plasticity and/or forming behavior, texture, firing color and character, thermal expansion and other properties are affected. It is a matter of accommodating a new material while maintaining the needed properties in the body. For example, to substitute a plastic ball clay a combination of a less plastic one with a bentonite addition might be the most suitable. Where a body's fired color depends on an iron-bearing clay, the substitute faces the challenge of not only imparting the same color, but also the same plasticity and fired maturity (thus a multimaterial approach is almost always needed).

Related Information

Substitute Ferro Frit 3134, using glaze chemistry, in three glaze types


Insight-live screen shot, substituting frit 3134

This picture has its own page with more detail, click here to see it.

Can't get frit 3134 for glaze recipes? Can you replace it with frit 3124? No, 3124 has five times the amount of Al2O3 (the second most important oxide in glazes) and half the amount of B2O3 (the main melter). This ten-minute video presents a glaze chemistry approach that is easier to do than you probably think. It deals with three different glaze recipe types lacking sufficient clay to suspend the slurry. Learn to source the needed oxides from two other Ferro frits, 3110 (or Fusion F-75) and 3195 (Fusion F-2), and end up with at least 15% kaolin in each. A unique approach is required in each situation. Two of the calculations produce improved slurry properties and one yields a recipe of significantly lower cost. If you have a recipe that needs this and need help please contact us.

Is Ferro Frit 3124 a viable substitute for Frit 3134?


Three melt from tests comparing these frits

This picture has its own page with more detail, click here to see it.

This is a GLFL test comparing the melt flow of the three materials at 1800F. Frit 3124 is barely out of the starting gate and the other two have crossed the finish line! With frits chemistry is a big deal, they are all about supplying oxides to the melt. Frit 3134 is low-alumina/high-boron, 3124 is medium-alumina/low-boron and 3195 is medium-alumina/high-boron. Boron is the melter. Alumina thickens the melt and hardens the glass. Just from this it appears that Frit 3195 is a better starting point for calculations to replace frit 3134.

Calculating a substitute for Minspar


Melt flow tests comparing the two felspars

This picture has its own page with more detail, click here to see it.

Why do this? We did not have it in stock and customers needed to mix recipes. When the chemistries of the two feldspars are very similar substitution is often not a problem, especially when a recipe only calls for 5 or 10%. However, when a recipe calls for a significant percentage the situation becomes much trickier (in our cone 6 test recipe, "Perfect Clear", 40% Minspar is needed). Feldspars are almost a glaze in themselves, just needing silica and alumina to shift their chemistry toward 'glazedom'. In this project I calculated a mix of materials, in my Insight-live.com account, that sources the same chemistry as Minspar. I made cone 6 GLFL tests comparing the pure Minspar and Minspar substitute (left) and comparing the Perfect Clear glaze with each feldspar (right). As you can see, the similarity in melt flow is stunning! This is a good demonstration of just how practical and valuable glaze chemistry calculation can be.

Which is the champion melter of American/Canadian feldspars?


Feldspars melting

This picture has its own page with more detail, click here to see it.

Feldspars are employed in glaze recipes as melters. So comparing their melt fluidities should be helpful in deciding if one can substitute for another (of course, if possible, a soda-predominant feldspar should be substituted for another soda spar). Feldspars don't melt alone at cone 6 (2200F) so we mixed each with 15% Ferro Frit 3195 (we consider a feldspar a material that sources KNaO). Nepheline Syenite, this is A270, is the champion melter here. Other similar ones can be spotted easily. In the end, degree of melt is a valid consideration in determining if one feldspar is a viable substitute for another in a recipe. Even if the feldspar you want to substitute does not melt as much a little frit can be added to the recipe to make up for the difference (e.g. 3-5%).

Arbuckle Majolica glaze using Fusion Frit F-19


Majolica glaze tiles

This picture has its own page with more detail, click here to see it.

Fusion Frit F-19 is said to be a substitute for Ferro Frit 3124, for this particular glaze that appears to be true. The Arbuckle Majolica glaze was applied on Plainsman L210 and fired at cone 04 (but not as thickly applied as would be customary on Majolica ware). On the left is the one with Ferro Frit 3124, on the right is the one with the F-19. The recipe is based on Ferro Frit 3124 and adds 20% of a feldspar neheline mix (likely to increase thermal expansion because it shivered on the original clay body). It is suspended by 10% kaolin. This may craze on your clay body, the G1916Q thermal expansion adjustable transparent base might be a better solution (it responds similarly to a zircon/tin addition to opacify).

G2934 using Fusion Frit F-19 instead of Ferro 3124


Melt fluidity tester comparing two versions of G2934

This picture has its own page with more detail, click here to see it.

G2934 is a popular recipe and there has been alarm recently because of the difficulty in getting the Ferro frit and the variation in its quality in recent years. This motivated us to get a supply of the Fusion equivalent, F-19. When doing substitutions like this we do testing in glazes and with melt fluidity tests - like this GLFL test.

Grolleg vs New Zealand - Which kaolin is better for translucency?


Two translucent mugs

This picture has its own page with more detail, click here to see it.

The NZK body, Polar Ice, is on the left. The Grolleg one, L3778D, is on the right. They are not the same recipe, the feldspar content in the L3778D has been adjusted to match the degree of vitrification (Grolleg contains some feldspar). Clearly, the NZK has better translucency. And it fires whiter.

Laguna Barnard Slip substitute fired bars


This picture has its own page with more detail, click here to see it.

These are fired bars of Laguna SG758 Barnard Slip substitute going from cone 04 (bottom) to cone 6 (top). It is melting at cone 6. The bars are expanded above cone 6 and becoming quite porous. The drying shrinkage is around 7%, it is quite plastic.

L3617 Cornwall Stone substitute vs. real Cornwall Stone


This picture has its own page with more detail, click here to see it.

This melt fluidity comparison demonstrates how similar the substitute L3617 recipe (left) is to the real material (right). 20% Frit 3134 has been added to each to enable better melting at cone 5 (they do not flow even at cone 11 without the frit). This substitute is chemically equivalent to what we feel is the best average for the chemistry of Cornwall Stone.

Comparing two brands of calcium carbonate


This picture has its own page with more detail, click here to see it.

This GLFL test compares the melt flow, at cone 6, of two glaze recipes containing the calcium carbonates (of which they make up 27%). Notice the amount of bubbles (due to the high LOI, or loss on ignition). The 3HX is flowing a little more. This could be because of a difference their proportions of dolomite and calcium carbonate minerals, the individual mineral purities or the particle size (or all three). Whatever the case, 3HX will make a glaze flow a slightly better.

Testing two brands of tin oxide in a melt flow tester


Tin oxide opacified glaze in a melt fluidity tester

This picture has its own page with more detail, click here to see it.

This melt fluidity tester compares two different tin oxides in a cone 6 transparent glaze (G2926B). Opacifiers affect not just opacity in glazes, but also liquid properties of the melt. The length, surface character, opacity and color of these flows provide an excellent indication of how similar the two materials are. This is the GLFL test.

Testing a new brand of dolomite


Melt fluidity of high dolomite glaze

This picture has its own page with more detail, click here to see it.

Dolomite is a key material for glazes, especially mattes. We were forced to adopt a new brand and needed confidence it was equivalent. Three tests were done to compare the old long-time-use material (IMASCO Sirdar) with a new one (LHoist Dolowhite). The first melt flow tester compares them in a very high dolomite cone 6 recipe formulated for this purpose; the new material runs just slightly more. The second tester is uses the G2934 cone 6 magnesia matte recipe with 5% black stain; the new material runs a little less here. The third test is the high dolomite glaze on a dark burning clay to see the translucency and compare the surface character. They are very close. These three gave us the confidence to proceed.

The difference between Silica 90 and Silica 45 will affect the glaze melt


This picture has its own page with more detail, click here to see it.

Quartz particles have a high melting point, they must enter the glaze melt by being dissolved by it (usually the last particles to do so). Obviously, the silica should be as fine as possible to increase its surface area to be more readily dissolved. The more that dissolves the closer the physical properties of the fired glaze will be to the theoretical (e.g. degree of melting, thermal expansion, transparency, durability). This brand of silica, #90 classifies as 200 mesh even though 2.8% remains on the 200 mesh screen. Not surprisingly, their #45 grade retains 1.9% on the 325 mesh screen. However, the most significant aspect is how much of the #90 is on the 325 and 270 mesh screens: 26%. The #45 grade only retains 2.6% on them! This is a huge difference and shows the value of using the finer material. It would take a typical ball mill hours to make this difference.

Redart (left) vs. Lizella clay. Definitely not substitutes for each other.


This picture has its own page with more detail, click here to see it.

These bars have been fired at cones 4, 2, 02, 04 (top to bottom) using the SHAB testing procedure. We can measure fired shrinkage and porosity in each to get an indication of their fired maturity. The Redart (left) is much more vitreous and reaches almost zero porosity by cone 4 whereas the Lizella still has 11% porosity at cone 4. Lizella also has a much higher drying shrinkage (because it is way more plastic).

Links

Glossary Ceramic Material
Ceramic materials are employed in the ceramic industry to make glazes, bodies, engobes and refractories. We study them at the mineral, chemical and physical levels.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy