0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Pinholing

Pinholing is a common surface defect that occurs with ceramic glazes. The problem emerges from the kiln and can occur erratically in production.

Key phrases linking here: pinholing, pinholes, pinhole - Learn more

Details

A glaze defect where tiny holes are present in the fired glaze surface. These holes normally go down to the body surface below. Pinholing is a plague in industry, the tiniest hole in the glaze surface of a tile or utilitarian item can make it a reject. Industry goes to great pains to get materials of very fine particle size for their bodies and glazes to reduce the occurrence of glaze defects. They need to be sure that ware can survive their fast firing schedules.

Glazes that melt and flow well often still have pinholes if gas producing particles are present in the body (these expel gases up through the glaze melt thereby disturbing its surface). Thicker layers of glaze pinhole more than thinner ones. Blisters, dimples and pinholes often occur together. Fast firing produces more pinholes.

Potters and smaller operations have a universal solution that manufacturers do not: The freedom to use drop-and-hold and slow-cool firing schedules, these can produce a perfect glaze surface on almost any clay body. Reduction gas firing is known to produce much fewer glaze defects, the reason is often that the kiln, because of its mass, cools much slower.

Some glaze chemistries are much more prone to pinholing. For example, high Al2O3 and ZrO3 stiffen the glaze melt making it less able to heal defects.

Related Information

Let me count the reasons this glossy white cone 6 glaze is pinholing


This picture has its own page with more detail, click here to see it.

First, the layer is very thick. Second, the body was only bisque fired to cone 06 and it is a raw brown burning stoneware with lots of coarser particles that generate gases as they are heated. Third, the glaze contains zircopax, it stiffens the melt and makes it less able to heal disruptions in the surface. Fourth, the glaze is high in B2O3, so it starts melting early (around 1450F) and seals the surface so the gases must bubble up through. Fifth, the firing was soaked at the end rather than dropping the temperature a little first (e.g. 100F) and soaking there instead.

One fired flawless, the other dimpled and pinholed.

These are the same glaze/body. Why?


This picture has its own page with more detail, click here to see it.

The difference is a slow-cool firing. Both mugs are Plainsman M340 and have the L3954B black engobe inside and partway down on the outside. Both were dip-glazed with the GA6-B amber transparent and fired to cone 6. The one on the right was fired using the PLC6DS drop-and-hold schedule. That eliminated any blisters, but some pinholes remained. The one on the left was fired using the C6DHSC slow-cool schedule. That differs in one way: It cools at 150F/hr from 2100F to 1400F (as opposed to a free-fall). It is amazing how much this improves the brilliance and surface quality (not fully indicated by this photo, the mug on the left is much better).

Solving a pinholes problem with a boron fluxed cone 04 opacified and stained glaze


This picture has its own page with more detail, click here to see it.

This problem was suffered by a potter moving from Europe to Canada. In Europe she used lead based glazes and got smooth defect-free surfaces. But in Canada she began using our Gerstley Borate based glazes and had many problems adapting to them. We used glaze chemistry to both adjust recipes to source boron from frits instead of GB and to reduce their melt fluidity. She also adjusted firings: Higher bisque and glaze firings and a drop-and-hold firing schedule (like C03DRH). And she adopted a finer particle-sized terra cotta clay body. These measures enabled her to eliminate the issue.

Pinholes often happen on trimmed surfaces


This picture has its own page with more detail, click here to see it.

Pinholing is often related to the smoothness of the underlying body surface. The lower half of this vase was tooled during the leather hard stage, all the pinholes occur there. Even though this body contains 10% grog, the pinholes are not appearing on the upper half because the slip generated during throwing has left a smooth surface.

What if you just cannot solve a pinhole problem?


This picture has its own page with more detail, click here to see it.

Pinholing on the inside of a cone 6 whiteware bowl. This is glaze G2926B. The cause is likely a combination of thick glaze layer and gas-producing particles in the body. Bodies containing ball clays and bentonites often have particles in the +150 and even +100 mesh sizes. The presence of such particles is often sporadic, thus it is possible to produce defect-free ware for a time. But at some point problems will be encountered. Companies in large production need to have fast firing schedules, so they either have to filter press or wet process these bodies to remove the particles. Or, they need to switch to more expensive bodies containing only kaolins and highly processed plasticizers. But potters have the freedom to use drop-and-hold or slow-cool firing schedules, that single factor can solve even serious pinholing issues.

Oversize particles in a typical manufactured porcelain body


This picture has its own page with more detail, click here to see it.

Example of the oversize particles from a 100 gram wet sieve analysis test of a powdered sample of a porcelain body made from North American refined materials. Although these materials are sold as 200 mesh, that designation does not mean that there are no particles coarser than 200 mesh. Here, there are significant numbers of particles on the 100 and even 70 mesh screens. These contain some darker particles that could produce fired specks (if they are iron and not lignite); thank goodness in this case they do not. Oversize particlate is a fact of life in bodies made from refined materials and used by potters and hobbyists. Industrial manufacturers (e.g. tile, tableware, sanitaryware) commonly process the materials further, slurrying them and screening or ball milling; this is done to guarantee defect-free glazed surfaces.

How can you best tell if a base glaze is prone to pinholing with your body?


This picture has its own page with more detail, click here to see it.

Testing for pinholes and dimples is often best done using a transparent glaze over a large surface and looking at the surface in the light. In this case, an open bowl is used. Heavy pieces like this are difficult to fire evenly and encourage under fired areas where pinholes are more likely to appear.

Cone 6 glazes can seal the surface surprisingly early - melt flow balls reveal it


This picture has its own page with more detail, click here to see it.

These are 10 gram balls of four different common cone 6 clear glazes fired to 1800F (bisque temperature). How dense are they? I measured the porosity (by weighing, soaking, weighing again): G2934 cone 6 matte - 21%. G2926B cone 6 glossy - 0%. G2916F cone 6 glossy - 8%. G1215U cone 6 low expansion glossy - 2%. The implications: G2926B is already sealing the surface at 1800F. If the gases of decomposing organics in the body have not been fully expelled, how are they going to get through it? Pressure will build and as soon as the glaze is fluid enough, they will enter it en masse. Or, they will concentrate at discontinuities and defects in the surface and create pinholes and blisters. Clearly, ware needs to be bisque fired higher than 1800F.

Lignite contamination in manufactured porcelain body


This picture has its own page with more detail, click here to see it.

These contaminating particles are exposed on the rim of a bisque-fired mug. The liqnite ones have burned away but the iron particle is still there (and will produce a speck in the glaze). Remnants of the lignite remain inside the matrix and can pinhole glazes. Since ball clays are air floated (a stream of air takes away the lighter particles and the heavier ones recycle for regrinding) it seems that contamination like this would be impossible. But the equipment requires vigilance for correct operation, especially when there is pressure to maximize production. Ores in Tennessee are higher in coal than those in Kentucky. North American clay body manufacturers who confront ball clay suppliers with this contamination find that ceramic applications have become a very small part of the total ball clay market - complaints are not taken with the same seriousness as in the past.

I once tolerated this amount of pinholing:

Then I discovered drop-and-hold firing


A cone 6 blue silky matte glazed vase with thousands of pinholes in the glaze

This picture has its own page with more detail, click here to see it.

This cone 6 vase was made from a coarse-grained stoneware body typical of those long produced by Plainsman Clays. These materials performed exceptionally well at cone 10 reduction, but when similar bodies began being fired at cone 6 oxidation, pinholing often became a challenge. Why? The coarser particle structure creates fewer but larger pathways for escaping decomposition gases, concentrating gas flow through localized vents and leaving behind pits like those visible here.

Yet today many potters fire these same clays with little or no pinholing. Electronic kiln controllers deserve much of the credit, making drop-and-hold and slow-cooling schedules practical. Equally important, I formulate glazes with enough melt fluidity to heal gas-release craters during the hold, while maintaining sufficiently low surface tension to avoid trapping gases in bubbles that later become blisters. Commercial glaze manufacturers have quietly optimized for these same properties.

Serious pinholing in pottery glaze:

Slow-cool the firing or get a different body.


Glaze pinholing on a pottery mug

This picture has its own page with more detail, click here to see it.

This cone 6 pottery glaze has high melt fluidity. But that is not enough to enable healing of these pinholes. This is Plainsman Coffee clay. It contains particle sizes up to 42 mesh, as some of those decompose near cone 6. As they do so, they expel gases that can concentrate enough at a single point on the surface that not even this glaze can cover the holes left. We normally resolve this using a drop-and-hold firing. For people unable to program the cooling curve of the firing schedule, bodies like this are not likely suitable unless glazes are tested to have the needed melt fluidity and surface tension to heal the pinholes.

Inbound Photo Links



Encapsulated stain orange-peels the glaze? Why? What can be done?


Pinholing at a cone 6 stoneware mug. Why?


One small pinhole in a terra cotta mug and we have a problem

And Insight-Live screenshot
What can you do using glaze chemistry? More than you think!

A chart showing weight-loss vs firing temperature for common ceramic materials
LOI horse race with surprising winners


Same cone 6 glazes. Same clay. Why is the one on the right pinholing?


Why is this cone 10 oxidation iron-brown glaze pinholing?

Links

Glossary Drop-and-Soak Firing
A kiln firing schedule where temperature is eased to the top, then dropped quickly and held at a temperature 100-200F lower.
Media Manually program your kiln or suffer glaze defects!
To do a drop-and-hold firing you must manually program your kiln controller. It is the secret to surfaces without pinholes and blisters.
Media A Broken Glaze Meets Insight-Live and a Magic Material
Use Insight-Live.com to do major surgery on a feldspar saturated cone 10R glaze recipe with multiple issues: blistering, pinholing, crazing, settling, dusting and possibly leaching!
Troubles Glaze Pinholes, Pitting
Analyze the causes of ceramic glaze pinholing and pitting so your fix is dealing with the real issues, not a symptom.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved