0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Formula | Oxide Interaction | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Stull Chart

Stull charts attempt to explain graphically, on an x-y coordinate system, specific fired properties of selected mixes of oxides. It is a visual way to understand the relationships between glaze chemistry and fired results. For example, a graph may display results for a constant amount of flux with varying amounts of SiO2 and Al2O3 (the latter corresponding to the x and y of the graph). Annotations typically highlight zones having specific properties (e.g. matteness, gloss, crystallization, etc). The focus of a chart must be clearly understood for it to be valid and valuable.

Chazo Chazim Mehmeti, who developed the UMF Glaze Excel stull chart creator says this (slightly edited):

My opinion, based on years of teaching, is that the Stull chart is the best in the history of glaze help. Why? Definitely not because Stull's chart is flawless. It's not! But people perceive a position on the graphic (map) much more easily than imagining where a glaze "falls" in a bunch of numbers. My students make comments like this: "Making glazes with the Stull chart and CBC has become a very interesting video game."
-First of all, users more easily understand the role of the fluxes in the glaze. By adding one they see how "the point" immediately drops.
-Advanced users can see the difference in the same gram amount of BaO vs. Li2O and better understand the role of molecular weight.
-Users more easily understand the composition of kaolin when the point moves diagonally upwards as a product of kaolin having more silica than alumina.
As already mentioned, there is no chart that can be exchanged for knowledge, but still, Stull charts are extremely helpful tools. In my spreadsheet I also have a chart I call "Chazo's Boron Curve", I developed it with some help from two of my friends (Prof. Dr. Sc. David Brčić, and Dr Sc. Viktor Bojović). I created the "CBC" to improve the precision of the Boron line (especially at low temperatures, eg. cone 04).


Generating Stull Charts requires a lot of organized testing and record keeping. An account at insight-live.com is one way to do that.

Related Information

Stull chart showing the SiO2-Al2O3-(0.7CaO+0.3KNaO) system


This picture has its own page with more detail, click here to see it.

The original Stull chart - Chart 1 from Transactions of the American Ceramic Society, Vol. XIV (1912). Stull mapped test glazes by their SiO2:Al2O3 molar ratio and identified the regions that predict surface quality.

If you really want to "get into the weeds" of glaze chemistry, the https://stullatlas.app tool, by Ryan Lack, takes Stull's insight and applies it to a modern dataset of real-world glazes, giving you an interactive map of the glaze chemistry landscape. The primary dataset comes from Glazy. It contains thousands of community-contributed recipes with calculated UMF values, cone temperatures, surface types, and firing atmospheres. Each point on the chart represents a real glaze recipe that someone has mixed, fired, and documented.

Why does fluid-melt G3948B not produce an iron red


Stull chart for iron red glazes

This picture has its own page with more detail, click here to see it.

Chazo Chazim Mehmeti made this Stull chart to help explain why my G3948B does not produce iron crystals. It plots the formula amounts of Al2O3 (vertical axis) vs. SiO2 providing one lens through which to view the chemistry of multiple iron red glaze recipe candidates that work and don't work. His argument is that, among other necessary things like the presence of P2O5, MgO and CaO, the amounts of SiO2:Al2O3 must be within certain bounds (this chart conveys both the ratio and amounts). He points out that the relationship is sensitive enough that one should use the closest possible chemical analysis of the materials (not generic ones) when plotting points on the chart. Over a year of testing with his students, the ones fitting in the small zone on the chart worked every time (#2 being best). That is where my G3948A, which is working really well, also resides. The G3948B, which does not work, appears way off to the right because of its high SiO2 content. Of course, there could be other reasons for its failure, but the SiO2 issue is a good place to start.

Links

Glossary Phase Diagram
URLs https://wiki.glazy.org/t/understanding-the-stull-chart/857.html
Understanding Stull Charts by Pieter Mostert
URLs https://stullatlas.app/#/about
Stull Atlas - A Computational Ceramic Glaze Explorer - 114 years after Stull
Stull Atlas is a tool for ceramic artists and glaze chemists. It lets you explore thousands of glaze recipes mapped onto a Stull chart - the standard coordinate system for understanding glaze chemistry through Unity Molecular Formula (UMF).

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy