0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Rate | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Casting Rate

Casting rate describes how quickly a layer of clay builds against the mold surface during slip casting.

Key phrases linking here: casting rate - Learn more

Details

Casting rate describes how quickly a layer of clay builds against the mold surface during slip casting. In conventional plaster molds, capillary suction draws water from the slip, leaving a consolidated layer of particles behind. Water must then pass through this layer for more material to deposit. As the wall thickens, resistance to water movement increases and further buildup slows. Thus, twice the casting time does not produce twice the wall thickness. For practical comparisons, casting rate can be assessed by measuring the thickness produced in a fixed time or the time needed to reach a specified thickness.

Casting rate depends strongly on the permeability of the deposited layer. While influenced by particle size distribution, particle packing and the degree of deflocculation, the main factor is the nature of the clays used, especially their plasticity. Very fine plastic clays can provide excellent strength but form layers through which water moves slowly. Larger-particle clays, which are less plastic, can build thickness much faster. However, speed alone is not the objective: The cast must also develop enough strength and drying shrinkage to pull itself away from the mold as it shrinks. The formulation challenge is to obtain sufficient strength and reliable release while retaining good permeability.

Casting rate is a property of the slip-and-mold combination, not simply of the body recipe. A wet mold will obviously cast more slowly than a dry one. Ware shape and surface detail also affect casting time. A testing program should therefore record wall-building time, release time and the quality of the resulting ware under comparable conditions.

Related Information

Demonstrate casting-rate control:

By slip-casting nepheline syenite


Nepheline syenite bowl

This picture has its own page with more detail, click here to see it.

What would it take to cast pure Nepheline Syenite? A clay addition. This 10:90 bentonite:Nepheline has enough shrinkage and leather-hard strength to enable pulling itself away from the plaster mold. This bowl was just extracted; it cast without cracks to 3mm thickness in about 15 minutes. The defloculated slip required more water than normal but it pours and drains really well. This is a demonstration of how much control technicians can have over casting rate. The amount and type of plastic clay added can take this material from being completely water permeable, zero leather-hard strength and non-castable to water impermeable, very high leather-hardness but very slow casting. Only a testing program is needed to determine the minimum bentonite percentage needed to achieve reliable casting (it is likely less than 10%).

For example, 95%+ nepheline slurries can be made using Veegum. How did this bowl fire? As a vitreous product around cone 1. And, on aging for a month, the rheological properties of the slurry did not change.

NZ kaolin-based slip casts at 1mm thickness. How?


A very thin walled porcelain bowl

This picture has its own page with more detail, click here to see it.

This is Polar Ice casting, a cone 6 translucent porcelain that uses New Zealand Halloysite. The base body recipe would never have enough plastic strength to pull itself from this mold without tearing. But the addition of 1% Veegum gives it amazing strength. This dried cast bowl measures 130mm in diameter and 85mm deep; it only weighs 89 gm! The slip was in the mold for only 1 minute before pour-out. Of course, there is a price to pay for adding the Veegum: Increased casting time and more difficult deflocculation. This 1% addition can be refined. A program of testing could indicate that a lower percentage of Veegum could work, increasing the casting rate. The polar ice information page has very good information, under the heading “Casting Recipe” (it deals with the trade-offs of using this kaolin in casting bodies).

This Cone 6 Porcelain Casts Super-Fast

The type of kaolin and ball clay is the secret


A small cast beer bottle still in the mold

This picture has its own page with more detail, click here to see it.

Rather than L4807 being just another cone 6 porcelain casting slip recipe it is a pattern of the flexibility potters/hobbyists could have in making their own bodies. This has incredible casting speed. If someone tells you that porcelains are always difficult to cast, tell them it’s time to go DIY.

Typical slips made from ball clay and talc (or mixes of common feldspars, clays and quartz) take 20-30 minutes to get the needed thickness (in our circumstances and assuming a new dry mold). But this one poured out in 12 minutes and I can demold in 10 minutes. The secret is not the recipe, this is similar to a typical 25-porcelain. The secret here is choice of kaolin and ball clay. This employs OptiKast Kaolin and KT#1-4 ball clay, both are large particled clays targeted at slip casting. They can be traded off for each other, more ball clay imparts better leather-hard strength but casts slower, more kaolin does the opposite. This is one more reason to mix your own casting bodies.

How a kaolin and ball clay compare in a dry performance test


This picture has its own page with more detail, click here to see it.

These are DFAC drying performance disks of a large-particle kaolin (OptiKast) and a ball clay (Plainsman A2). This test reveals a clay's response to uneven drying (these disks are dried with the center portion covered). The kaolin feels smoother yet its ultimate particles are ten to one hundred times bigger than a typical ball clay. Thus it shrinks much less. The ball clay has dramatically lower water permeability, water from the center protected portion resists migration to the outer edge during drying. When the inner section finally dried the outer was already rigid so it split the disk in two and pulled all the edge cracks. Most ball clays shrink more and crack worse than this (cracks concentric to the center also appear). So why use ball clay? This kaolin is so lacking in plasticity it was barely possible to even make this disk. And it is so weak that it can easily break just by handling it. Still, it is useful to make casting bodies. But the ball clay, when used as a percentage of a body mix, can produce highly plastic bodies than can be dried without trouble if done evenly.


PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy