0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Boron Blue

Boron blue is a glaze fault involving the crystallization of calcium borate. It can be solved using glaze chemistry.

Key phrases linking here: boron blue, boron-blue - Learn more

Details

Boron blue is the bluish haze or clouding in a transparent boron glaze that results from the crystallization of calcium borate in the glass matrix during cooling. While the effect might be considered decorative in some cases, this is generally considered a glaze fault. It is a common problem in high boron glazes, the higher the CaO the worse it is. It is about the chemistry of the glaze (even though some might like to blame the frit).

If possible, try cooling faster (of course there is a risk for dunting with this approach). That gives the crystals less time to grow. Or, by firing tests it might be possible to isolate the temperature range where it happens and just cool quickly through that.

The most effective approach is to reduce the CaO. As long as it is not excessive the crystals should not form. Even if the glaze has plenty of boron.

If the glaze is melting well it will likely tolerate the addition of more Al2O3. Increasing it without changing anything else impedes the growth of crystals (by stiffening the melt thereby denying the molecules the mobility they need to form the preferred crystalline arrangement). There are added benefits to this also (e.g. better hardness, lower expansion).

These changes are done using glaze chemistry. If you enter a recipe into your account at Insight-live.com it can show you the amount of each oxide (e.g. CaO, Al2O3, SiO2) and you can click materials to see what oxides they contribute. Then duplicate the recipe to view it side-by-side with the original. Adjust ingredients and note the impact on the chemistry. It may be as simple as changing some or all of an existing frit for another frit (or mix of frits) having higher Al2O3 and a mix of fluxes having a lower percentage of CaO. A common way to add Al2O3 is to increase the kaolin and reduce the silica (to re-match the SiO2).

The most non-technical way to adjust the recipe is to simply blindly try other frits. While this might reduce the boron blue, the different chemistry they bring will affect other properties (like color response, thermal expansion, melting temperature, hardness and durability, surface character, matteness or gloss). Since the root problem is with two oxides the best approach is to focus on them.

Boron blue can also be used as a decorative effect, especially on low-temperature ware. To encourage it just do the opposite of everything mentioned above.

Related Information

Boron blue in low fire transparent glazes


This picture has its own page with more detail, click here to see it.

This high-boron high-CaOcone 04 glaze is generating calcium-borate crystals during cool down (called boron-blue). This is a common problem and a reason to control the boron levels in transparent glazes; use just enough to melt it well. If more melt fluidity is needed, decrease the percentage of CaO in favor of a lower melting oxide, that will certainly help. There is a positive: For opaque glazes, this effect can actually enable the use of less opacifier.

A severe case of boron blue creates opalescence


Opalescent glaze brings issues

This picture has its own page with more detail, click here to see it.

So-called opal or opalescent glazes are commonly ones having a combination of boron blue coupled with plenty of titanium or rutile to enhance the effect. However such glazes bring along significant "baggage". For example, 6-7% titanium, which, on cooling in the kiln, would matte or crystallize many glazes, can be tolerated because of the high melt fluidity. Unfortunately runny glazes bring issues for production. And, glazes of this type commonly have a high percentage of feldspar (to source the needed KNaO), unfortunately that means they will craze. Plus, the high melt fluidity needed for the effect requires a low percentage of Al2O3. That has other implications. First, hardness of the fired glaze is affected. Second, since Al2O3 is being contributed by the feldspar, there is no room left in the recipe for kaolin or ball clay (which normally sources the Al2O3). In the past, Gerstley Borate, a very active melter that is also plastic was an ideal solution. Unfortunately, Gillespie borate, the recommended substitute, does not have the same suspending properties. One solution is to source the KNaO from Ferro Frit 3110, using glaze chemistry. It has almost no Al2O3 so significant kaolin can be added to source it. However, that still does not fix the issue of crazing. An alternate solution is to find another melt fluid lower expansion base glaze and add the titanium to that.

Why would a low fire transparent require four frits?


This picture has its own page with more detail, click here to see it.

To get the needed chemistry to avoid boron blue clouding (calcium borate crystals). The one on the right clouds, the other does not. Why? Differences in the chemistry (as seen in my account at insight-live.com). G2931K, on the left, has greater Al2O3 (which impedes the growth of crystals), lower CaO (starves their growth) and more boron (for better melting). There is actually no practical way to adjust the recipe on the right (by supplying MgO with talc and fiddling with frit percentages) to achieve this. Frit 3124 lacks Na2O and B2O3. 3134 has excessive CaO and almost zero Al2O3. Talc does not melt well enough. But Frit 3249 supplies the needed MgO and has lots of B2O3 and low CaO. And Frit 3110 has low CaO and supplies the needed Na2O.

What happens when ceramic glazes lack Al2O3?


This picture has its own page with more detail, click here to see it.

This happens. They are glossy, but lack thickness and body. They are also prone to boron blue clouding (micro crystallization that occurs because low alumina melts crystallize much more readily on cooling). Another problem is lack of resistance to wear and to leaching (sufficient Al2O3 in the chemistry is essential to producing a strong and durable glass). This is a good example of the need to see a glaze not just as a recipe but as a chemical formula of oxides. The latter view enables us to compare it with other common recipes and the very low Al2O3 is immediately evident. Another problem: Low clay content (this has only 7.5% kaolin) creates a slurry that is difficult to use and quickly settles hard in the bucket.

What has this low fire transparent glaze turned blue?


This picture has its own page with more detail, click here to see it.

It is made from 85% Ferro Frit 3134, 7.5% kaolin and 7.5% silica. While not obvious from the recipe, one look at the chemistry of this (as displayed when you enter a recipe into your account at insight-live.com) will show very low Al2O3. Frit 3134 has almost no Al2O3, yet it is an essential component of functional glazes (for durability, resistance to crystallization, stability during firing). The kaolin is the only contributor of Al2O3 and there is only a little. A simple fix would be to use Ferro Frit 3124 instead, remove the silica and increase the kaolin to 15.

The perfect storm to create boron-blue clouding at low fire


This picture has its own page with more detail, click here to see it.

Two clear glazes fired in the same slow-cool kiln on the same body with the same thickness. Why is one suffering boron blue (1916Q) and the other is not? Chemistry and material sourcing. Boron blue crystals grow best when there is plenty of boron (and other power fluxes), alumina is low, adequate silica is available and cooling is slow enough to give them time to grow. In the glaze on the left B2O3 is higher, crystal-fighting Al2O3 and MgO levels are a lot lower, KNaO fluxing is significantly higher, it has more SiO2 and the cooling is slow. In addition, it is sourcing B2O3 from a frit making the boron even more available for crystal formation (the glaze on the right is G2931F, it sources its boron from Ulexite).

Inbound Photo Links


Boron blue on a black stoneware body
This boron blue effect depends on three things: A dark body, variations in thickness, the right chemistry

A glaze eats though a firebrick
A pottery glaze that can eat through a firebrick!

Links

Oxides Al2O3 - Aluminum Oxide, Alumina
Glossary Glaze Chemistry
Glaze chemistry is the study of how the oxide chemistry of glazes relate to the way they fire. It accounts for color, surface, hardness, texture, melting temperature, thermal expansion, etc.
Glossary Crystallization
Ceramic glazes form crystals on cooling if the chemistry is right and the rate of cool is slow enough to permit molecular movement to the preferred orientation.
Glossary Opacity
Opacity of ceramics glazes is normally achieved by adding an opacifier like tin oxide or zircon. However, there are chemical profiles that can turn transparent glazes milky and make it cheaper to opacify them.
Glossary Transparent Glazes
Every glossy ceramic glaze is actually a base transparent with added opacifiers and colorants. So understand how to make a good transparent, then build other glazes on it.
Glossary Opacifier
Glaze opacity refers to the degree to which it is opaque. Opacifiers are powders added to transparent ceramic glazes to make them opaque.
Materials Gerstley Borate
Gerstley Borate was a natural source of boron for ceramic glazes. It was plastic and melted clear at 1750F. Now we need to replace it. How?
Recipes G1216M - Cone 6 Ultraclear Glaze for Porcelains
Substitute for low expansion cone 6 G1215U, this sources MgO from talc instead of a frit

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy