0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Cone 5

Also called "middle temperature" by potters, cone 5 (~2160F/1180C) refers to the low end of the temperature range at which most hobby and pottery stonewares and porcelains are fired.

Key phrases linking here: cone 5 - Learn more

Details

Many potters are moving from cone 6 (2200F or 1200C) down to cone 5 (2160F or 1180C). The energy savings by firing 40 degrees F lower is considerable and there is much less wear-and-tear on the elements in electric kilns (as kiln elements get old the kiln can really struggle to climb the last few degrees).

Conveniently, many middle temperature commercial glazes are targeted at the cone 5-6 range. Most cone 6 pottery glazes still melt well, especially with temperature holds at the end of firings. Test firing, especially using the C5DHSC schedule, will prove whether cone 6 glazes work. In many cases, especially with reactive glazes that are actually overfired at cone 6, better results will be obtained at cone 5.

However, making bodies mature a cone lower can be tricky. You cannot just use any cone 6 body and expect to make ware of the same durability at cone 5. White-burning bodies, where the feldspar percentage is already maxed-out to get them to vitrify at cone 6, are most impacted by firing them lower. Any cone 6 body that already has a significant porosity is only going to see it go higher at cone 5. That being said, a fully vitrified cone 6 porcelain easily qualifies as a white stoneware at cone 5. Buff burning bodies high in ball clay can be made to vitrify easily at cone 5 since there is plenty of room for extra feldspar. Brown and red burning bodies will lose color at cone 5. That being said, they are easiest of all to modify for cone 5 (and even lower) since they usually contain red-burning terra cotta clays that both plastify and flux the body, increasing the percentage of these moves the vitrification range downward. Producers that supply photos of the body color at many cones make assessment for cone 5 much easier.

Related Information

This cone 6 pottery clay is not suitable at cone 5? Why?


A red clay fired at 5 temperatures

This picture has its own page with more detail, click here to see it.

These SHAB test bars show this body fired from cone 8 (top) down to cone 4 (bottom). The test data indicates it reaches maximum firing shrinkage (FSHR column) at cone 7. Its porosity is 2.5% at cone 6 (ABS column), that is where red color is richest. By cone 5 it has reached 3.8%, that is pretty high for strong functional ware. At cone 7 the porosity is lower, 1.4%, but the color change indicates some decomposition is beginning (signifying possible issues with glaze bubbling, pinholes and warping of ware). Clearly, cone 6 is the most realistic temperature, it is still red and dense enough to have good strength and certainly won't leak if glazes are not crazed.

Firing one cone lower improves the glaze result


Two blue coffee mugs

This picture has its own page with more detail, click here to see it.

The mug on the left was fired to cone 6 using the PLC6DS drop-and-hold schedule. The one on the right was fired using the drop-and-hold slow-cool C5DHSC schedule. This is the same body, Plainsman M390. The most visible difference is the outside GR6-M glaze, it is turning out a little different at cone 5, firing a lighter less variegated blue. That being said, it sometimes turns out that way at cone 6 also, so there may be other factors. However, a more important difference is the inside glaze, L3500G. Notice how much more glassy and perfect it is. How is it possible to be so much better at cone 5 than cone 6? The slow-cool is the answer, that firing drops at 150F/hr from 2100F to 1400F.

The glossiest slipperiest glaze ever at middle temperature


Vase and bowl with super gloss glaze

This picture has its own page with more detail, click here to see it.

This is G3903, a variation on the GA6-B base Alberta Slip honey glaze for cone 6 (but these pieces are fired at cone 5). Its secret is Fusion Frit FZ-16 (high in both B2O3 and ZnO), this is the lowest melting frit we have ever seen. The 20% frit in this recipe is excessive for cone 6, likely 15% or even less would do. Even at cone 4 this glaze is super glossy. An amazing aspect is its slipperiness: Glazed test tiles of this cannot be stacked, they just slide off each other! Put a few coins in that bowl, move it around a little and they slide around and just fly right out! And, I must hold pieces tightly or they will slide out of my hands. Given that this glaze is 80% of a raw native clay and the pieces are made from M340S it is amazing that this small percentage of frit could produce such a brilliant surface. Notice also that it washes away the manganese speckle. Can you get this frit? No. Fusion Ceramics does not sell small quantities - despite many requests that they open a retail sales department for potters.

How I got a better matte black:

Cone 5 instead of 6


Three matte black pottery mugs

This picture has its own page with more detail, click here to see it.

In our electric kilns, cone 5 finishes at 2163F (vs cone 6 at 2200F). The bodies I normally use need cone 6 to vitrify to the degree I want. But not so with our MNP, it is vitreous at cone 5. And our black matte G2934BL glaze just happens to produce better matteness at cone 5, especially with the cone 5 C5DHSC firing schedule. The inside glaze is L3500G, it is melting just as well as at cone 6.

Cone 5 vs Cone 6 Polar Ice porcelain mugs


This picture has its own page with more detail, click here to see it.

The firing schedule for cone 5 was C5DHSC. The inside glaze is G2926B, outside is G2926B plus 10% Mason 6304 purple stain. There is no visible difference in the fired result.

The same oatmeal glaze on the same body at cone 5 and 6 oxidation


Two oatmeal glazed cone 6 mugs

This picture has its own page with more detail, click here to see it.

The outsides of these mugs are glazed using the G3933 recipe. Its speckle depends on the natural agglomeration that occurs in 200 mesh red iron oxide powder (the slurry was not ball millled or sieved so as not to break them up). Rutile and tin oxide are also present to help variegate the color. The body is M390, a red burning stoneware. At cone 6, using the C6DHSC schedule, the speckle is slightly more vivid in the one on the right. The drop-and-hold and slow-cool C5DHSC firing schedule used on the left helped develop the melt well even though the firing temperature is lower. The color also bleeds less across the color boundary on the lip at cone 5. The inside glazes are L3500G.

Inbound Photo Links



A silky matte oatmeal glaze recipe that is working very well at cone 5

Links

Glossary Cone 6
Also called "middle temperature" by potters, cone 6 (~2200F/1200C) refers to the temperature at which most hobby and pottery stonewares and porcelains are fired.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy