0.8mm thickness | 200 mesh | 325 mesh | 3D Design | 3D Modeling | 3D Printer | 3D Printing Clay | 3D Slicer | 3D-Printing | 42 mesh | A.I. in Ceramics | Abrasion Ceramics | Acidic Oxides | Agglomeration | AI at Digitalfire | Alkali | Alkaline Earths | All-in-one case mold | Amorphous | Apparent porosity | Artware | Ball milling | Bamboo Glaze | Base Glaze | Base-Coat Dipping Glaze | Basic Oxides | Batch Recipe | Bisque | Bit Image | Black Core | Bleeding of colors | Blender Mixing | Blunging | Body Bloating | Body glaze Interface | Body Warping | Bone China | Borate | Boron Blue | Boron Frit | Borosilicate | Breaking Glaze | Brick Making | Brushing Glaze | Calcia Matte | Calcination | Calculated Thermal Expansion | Candling | Carbon Burnout | Carbon trap glazes | CAS Numbers | Casting Slip | Casting-Jiggering | Catch Glaze | Celadon Glaze | Ceramic | Ceramic Binder | Ceramic Decals | Ceramic Glaze | Ceramic Glaze Defects | Ceramic Ink | Ceramic Material | Ceramic Oxide | Ceramic Slip | Ceramic Stain | Ceramic Tile | Ceramic Transfer | Ceramics | Characterization | Chemical Analysis | Chromaticity | Clay | Clay body | Clay Body Porosity | Clay Stiffness | Clays for Construction | Clays for Ovens and Heaters | Code Numbering | Coil pottery | Colloid | Colorant | Commercial hobby brushing glazes | Cone 1 | Cone 5 | Cone 6 | Cone plaque | Content Management System | Copper Red | Cordierite Ceramics | Crackle glaze | Creative Commons Attribution | Cristobalite | Cristobalite Inversion | CRM | Crucible | Crystalline glazes | Crystallization | Cuerda Seca | Cutlery Marking | Decomposition | Deflocculation | Dehydration | Differential thermal analysis | Digitalfire API | Digitalfire Foresight | Digitalfire Insight | Digitalfire Insight-Live | Digitalfire Reference Library | Digitalfire Taxonomy | Dimpled glaze | Dinnerware Safe | Dip Glazing | Dipping Glaze | Dishwasher Safe | Displacer | Do-It-Yourself | Drop-and-Soak Firing | Drying Crack | Drying Performance | Drying Shrinkage | Dunting | Dust Pressing | Earthenware | Efflorescence | Encapsulated Stain | Engobe | Eutectic | Fast Fire Glazes | Fat Glaze | FDM, SLA, SLS, MEX 3D printing technologies | Feldspar Glazes | Filter Press | Fining Agent | Firebrick | Fireclay | Fired Strength | Firing Schedule | Firing Shrinkage | Flameware | Flashing | Flocculation | Fluid Melt Glazes | Flux | Food Safe | Foot Ring | Forming Method | Formula Ratios | Formula Weight | Frit | Fritware | Functional | GHS Safety Data Sheets | GitHub | Glass vs. Crystalline | Glass-Ceramic Glazes | Glaze Blisters | Glaze Bubbles | Glaze Chemistry | Glaze Compression | Glaze Crawling | Glaze Crazing | Glaze Durability | Glaze fit | Glaze Gelling | Glaze laydown | Glaze Layering | Glaze Mixing | Glaze Recipes | Glaze shivering | Glaze Shrinkage | Glaze thickness | Globally Harmonized Data Sheets | Glossy Glaze | Green Strength | Grog | Gunmetal glaze | Hand Building Techniques | High Temperature Glaze | Hot Pressing | Incised decoration | Industrial clay body | Infill and Support | Ink Jet Printing | Inside-only Glazing | Iron Red Glaze | Jasper Ware | Jiggering | JSON | Kaki | Kiln Controller | Kiln Firing | Kiln fumes | Kiln venting system | Kiln Wash | Kneading clay | Kovar Metal | Laminations | Leaching | Lead in Ceramic Glazes | Leather hard | Limit Formula | Limit Recipe | Liner Glaze | Liner Glazing | Liquid Bright Colors | LOI | Low Temperature Glaze | Magnesia Matte | Majolica | Managed Service Provider | Marbling | Material Sense | Matte Glaze | Maturity | Maximum Density | MDT | Mechanism | Medium Temperature | Melt Fluidity | Melting Temperature | Metal Oxides | Metallic Glazes | Micro Organisms | Microwave Safe | Mineral phase | Mineralogy | Mocha glazes | Mohs Hardness | Mold Natches | Mold Shell Flange | Mole% | Monocottura | Mosaic Tile | Mottled | Native Clay | Non Oxide Ceramics | Oil-spot glaze | Once-Fire | Opacifier | Opacity | Ovenware | Overglaze | Oxidation Firing | Oxide Interaction | Oxide Molecular Formula | Oxide System | Particle classification | Particle orientation | Particle Size Distribution | Particle size reduction | Particle Sizes | PCE | Permeability | Phase Diagram | Phase Separation | Physical Testing | Pinholing | Plainsman Clays | Plaster Bat | Plaster table | Plasticine | Plasticity | Plucking | Porcelain | Porcelain Insulators | Porcelaineous Stoneware | Portable Document Format | Pour Glazing | Pour Spout | Powder Carrier | Powder Processing | Precipitation | Primary Clay | Primitive Firing | Propane | Propeller Mixer | Pugmill | Pyroceramics | Pyrometric Cone | Quartz Inversion | R2O:RO Ratio | Raku | Reactive Glazes | Reduction Firing | Reduction Speckle | Refiring Ceramics | Refractory | Refractory Ceramic Coatings | Representative Sample | Residual Quartz | Restaurant Ware | Rheology | Rutile Blue Glazes | Salt and Soda firing | Sanitary ware | Sculpture | Search Engine Optimization | Secondary Clay | Shino Glazes | Side Rails | Sieve | Sieve Shaker | Silk screen printing | Sintering | Slaking | Slip Casting | Slip Trailing | Slipware | Slurry | Slurry Processing | Slurry Up | Soaking | Soluble colors | Soluble Salts | Specific gravity | Splitting | Spray Glazing | Stain Medium | Stoneware | Stull Chart | Sulfate Scum | Sulfates | Surface Area | Surface Tension | Suspension | Tapper Clay | Tenmoku | Terra Cotta | Terra Sigilatta | Test Kiln | Theoretical Material | Thermal Conductivity | Thermal Expansion in Ceramic Bodies and Glazes | Thermal shock | Thermocouple | Thixotropy | Throwing | Tipping point | Tony Hansen | Toxicity | Trafficking | Translucency | Transparent Glazes | Triaxial Glaze Blending | Ultimate Particles | Underglaze | Unity Molecular Formula | Upwork | Variegation | Viscosity | Vitreous | Vitrification | Volatiles | Water Content | Water in Ceramics | Water Smoking | Water Solubility | Weathering of Clays | Wedging | Whiteware | WooCommerce | Wood Ash Glaze | Wood Firing | WordPress | Zero3 | Zero4 | Zeta Potential

Agglomeration

The fine mineral, oxide and clay particles used in ceramics often aglommerate during storage or even in the latter stages of production. These must be broken down later.

Key phrases linking here: agglomeration, agglomerates, agglomerate - Learn more

Details

In powders and slurries, particles can aggregate, sticking together with varying degrees of tenacity. Agglomerates can be thousands or even millions of particles. The mechanisms of the bonding can be physical, electrolytic or chemical. If measures are not taken to recognize and avoid the problem process and ware quality are detrimentally affected.

Fine powders used in ceramics often agglomerate during storage. Mixing equipment capable of injecting plenty of energy (e.g. a propeller mixer) can break these down (if used appropriately). Sieving is also helpful, the finer the mesh size the better the breakdown (however openings in even the finest sieves can still permit agglomerates of thousands or particles).

Pigment agglomerates can produce specking that can render ware unsaleable. Agglomerates in bodies, especially porcelains, will reduce fired strength and affect fired surface appearance and character. Agglomerates in slurries (casting bodies, engobes and glazes) will also are fired surface appearance. In slurries, the agglomerates are often the fine-particled clays - their presence implies the clay particles are not fully performing their suspending, hardening or gelling function.

Related Information

Wollastonite containing glazes should be sieved


This picture has its own page with more detail, click here to see it.

Screen a glaze to break down the wollastonite agglomerates (which often form in storage). This is an 80 mesh plastic sieve (the actual screen is a metal insert inside), I am using a spatula to encourage it to pass through the screen. If you do not do this, the small lumps you see on the freshly glazed piece will fire to surface bumps and ruin the glaze.

Agglomeration of New Zealand kaolin in both fritware body and glaze


White agglomerate flecking in a porcelain

This picture has its own page with more detail, click here to see it.

White agglomerates of New Zealand kaolin (NZK) have ruined both glaze and body (Zero4 fritware). Both were slurried up by propeller mixing (the latter dewatered on a plaster table). But in both cases, the action of our lab mixer, a very capable device, was not enough to break up the NZK agglomerates! The glaze appears to be the easiest to fix: Sieve it at 100 mesh. But does that really work? No. The particles are 10-20 times smaller than the openings so countless agglomerates could easily remain intact. The body is another matter. It is just about impossible to sieve because it contains significant VeeGum that gels the slurry. However, I am a potter and don't need to make thousands of gallons. Blender mixing is the answer, on high speed, it smashes the agglomerates in seconds. Even for many gallons it is easy to process the slurry in batches using the 2 litre jar of my mixer.

A wollastonite-containing glaze slurry not sieved


This picture has its own page with more detail, click here to see it.

This glaze has just been applied to a bisqued tile. It contains wollastonite, which can agglomerate in storage. It was propeller-mixed at high speed, but that was not enough to break down the white lumps (agglomerates). But they can be broken down by sieving the slurry through 80 mesh or finer. Other materials also behave in this manner (e.g. barium carbonate, iron oxide, cobalt oxide, clays, tin oxide, zircon, titanium dioxide). This being said, blender mixing would likely have broken these down.

The difference propeller-mixing makes in a titanium glaze


Titanium opacifies if mixed well

This picture has its own page with more detail, click here to see it.

The glaze has 5% added titanium dioxide. These were fired at cone 6. The titanium in the one on the left remained agglomerated, it did not disperse in the slurry during hand mixing (the agglomerates can be seen as white particles floating in the glass). On high-speed propller-mixing the effect on the right was produced! Blender mixing would be even better. This incredible difference occurs because the mixer is able to break up the titanium agglomerates, dispersing and wetting all the surfaces of the incredibly tiny particles. In this state they do their magic during the firing, opacifying and variegating the otherwise transparent base matte glaze. Would sieving be as good? Only partially, the particles are 200+ times smaller than the openings in an 80-mesh sieve, high energy input is needed to separate them.

Don't waste expensive tin oxide, propeller mix glazes well


Tin oxide in glaze needs thorough mixing

This picture has its own page with more detail, click here to see it.

This is a cone 04 glaze on a terra cotta body. Two 300-gram test batches were made. Both have 5% tin oxide added to a base transparent, G1916Q. The one on the left was high-speed propeller-mixed for 10 seconds. That was not enough, small agglomerates appear as tiny white specks floating in the glass. The one on the right was blender mixed for 60 seconds. Now the incredibly small tin particles have been dispersed and can do their job of opacifying the glaze. Would sieving the slurry have worked? No, the particle agglomerates can be far smaller than the openings in an 80-mesh sieve (individual particles could be 1000 times smaller!). The thorough dispersion of the expensive tin oxide particles has real benefit: It enables making an accurate assessment of whether the 5% addition is enough. In this case it isn't, more is needed.

This is how New Zealand kaolin powder agglomerates


This picture has its own page with more detail, click here to see it.

These lumps do not break down easily in a dry mixer, even when with other materials (like silica and feldspar). And they just bounce around on a vibrating screen. That means that without some sort of finishing device in the dry material feed stream is needed to break down these lumps before the pugmill.

Here’s how I make a base brushing engobe


Engobe mixing in a blender

This picture has its own page with more detail, click here to see it.

This brushing engobe has already passed my EBCT test for use on the intended body. It is thick and gooey (because it contains CMC gum), so it is practically impossible to sieve. My regular propeller mixer is not able to break up the tiny agglomerates of New Zealand kaolin. But 30 seconds of blender mixing makes it as smooth as silk. To make this liter of brushing engobe, I use 800g of powder and 10g of CMC gum in 800g of water. Because of the very high clay content, this does not require Veegum to gel it. The CMC gum greatly improves the brushing properties. It also thins the slurry enough to enable its lower-than-normal water content, making it more suitable for painting onto leather-hard ware, often in as little as one coat.

4% iron oxide in a clear glaze. Unscreened. The result: Fired specks.


This picture has its own page with more detail, click here to see it.

Iron oxide is a very fine powder. Unfortunately it can agglomerate badly and no amount of wet mixing seems to break down the lumps. However putting the glaze through a screen, in this case, 80 mesh, does reduce them in size. Ball milling would remove them completely. Other oxide colorants have this same issue (e.g. cobalt oxide). Stains disperse much better in slurries.

Comparing the fired glaze specks from different iron oxide brands


This picture has its own page with more detail, click here to see it.

Five different brand names of iron oxide at 4% in G1214W cone 5 transparent glaze. The glazes have been sieved to 100 mesh but remaining specks are still due to agglomeration of particles, not particle size differences.

Blue specks in a pugged porcelain. Be careful when adding stain.


This picture has its own page with more detail, click here to see it.

This is the cut-line on a wet, plastic slug of porcelain. These specks are agglomerates of a blue stain and existed even though the porcelain was dispersed under a powerful slurry mixer for ten minutes. Pure cobalt, if used to stain a porcelain, is known to do this. So stain is often used as an alternative. Some stains disperse much better than others (and do not agglomerate like this). The lesson is to test the colors of the stain available to you to make sure and use one that does disperse well.

Links

Glossary Dust Pressing
Many ceramic products, especially tile, are formed by pressing high-moisture or binder-containing dust or pelletized dust into steel molds at high pressures.
Glossary Propeller Mixer
In ceramic studios, labs and classrooms, a good propeller mixer is essential for mixing glaze and body slurries.
Glossary Ultimate Particles
Utlimate particles of ceramic materials are finer than can be measured even on a 325 mesh screen. These particles are the key players in the physical presence of the material.
URLs https://en.wikipedia.org/wiki/Particle_aggregation
Particle Agglomeration on Wikipedia

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy