| Monthly Tech-Tip | No tracking! No ads! |
Cone 03 white stoneware with red terra cotta ball-milled slip and transparent overglaze. They are L3685U engobe (Ferro frit 3110, #6 tile kaolin, Silica), near the final mix for a white low fire stoneware. The G1916J glaze is super clear. Why? Two reasons. These were fired in a schedule designed to burn off the gases from the bentonite in the body before the glaze fuses (it soaks the kiln for 2 hours at 1400F). Terra cotta clays generate alot of gases at cone 03 (producing glaze micro-bubbles), but here the terra cotta is only a thin slip over the much cleaner burning white body.
| Media |
How to Apply a White Slip to Terra Cotta Ware
I will show you some secrets of making a base engobe (or slip) apply to leather hard terracotta ware in a thick, perfectly even layer. |
| Recipes |
L3685U - Cone 03 White Engobe Recipe
A white burning body with enough added frit to produce a cone 03 stoneware or white slip for use on the matching red Zero3 stoneware. |