Black Coring
Bleeding Colors
Bloating
Casting Slip Problems
Chrome Flashing in Ceramic Glazes
Clouding in Ceramic Glazes
Cracking of Clays During Drying
Crawling
Dunting and Cracking of Clay Bodies During Firing
Foaming of Ceramic Glaze Slurries
Glaze Blisters
Glaze Crazing
Glaze is Off-Color
Glaze Marks or Scratches
Glaze peeling on drying
Glaze Pinholes, Pitting
Glaze Shivering
Glaze Slurry is Difficult to Use or Settling
Leaking of Fired Ceramics
Lime Popping
Orange Peel Surface
Over Firing of Ceramic Glazes and Bodies
Powdering, Cracking and Settling Glazes
Runny Ceramic Glazes
Specking on Ceramic Ware
Splitting at the Plastic Stage
Staining of Fired Ceramic Glazes
Uneven Glaze Coverage
Warping

Crawling

Ask yourself the right questions to figure out the real cause of a glaze crawling issue. Deal with the problem, not the symptoms.

Details

Crawling is where the molten glaze withdraws into islands, leaving bare clay patches between them. The edges of the islands are thickened and smoothly rounded. This is among the most common and costly problems in ceramic production. Ware requires refiring and is often lost anyway. In moderate cases there are only a few bare patches; in severe cases the glaze forms beads and even drips off onto the shelf. The problem is prevalent where dipping glazes are applied to bisque, shrink on drying and form cracks. This is usually because the glaze has excessive plastic clay content or is applied too thickly.

It is common to see this issue misdiagnosed on social media - someone submits a picture, and among the dozens of comments, no one asks about the recipe or mentions the factors noted below.

Is the glaze shrinking too much during drying?

If the dried glaze forms a network of cracks, it is a sign that the glaze is shrinking too much or its bond with the body is poor. The fault lines provide places for the crawling to start (especially where the island cracks delineate raised edges that are no longer in contact with the body). There are a number of possible contributors:

It is possible to create glaze slurries that gel and flow extremely well, dry hard and do not crack by using the right kaolin (i.e. EPK) or ball clay (i.e. Old Hickory #5, No. 5 Glaze) in adequate amounts. It is very important to realize that many ball clays and kaolins to not produce glazes of good slurry properties (without additives); a simple substitution can make a remarkable difference. It may not seem that glaze chemistry is related to this subject of getting the right type and right amount of clay in a recipe. But it very much is. Why? Because the ability to juggle a recipe to source Al2O3 from a clay or a feldspar/frit, as needed, enables controlling the amount of clay in the recipe while maintaining its fired character. Chemistry also gives you the ability to switch between different types of clay (that have different oxide makeups).

Is the glaze's dry-bond with the ware surface inadequate?

The mechanism of the bond between dry glaze and body is simply one of physical contact, the roughness of the ware surface copmbined with the ability of the liquid glaze to flow into all the tiny surface pores and irregularities and the degree to which it is able to dry hard without shrinking too much, these determine its ability to 'hang on'.

Does application technique or handling compromise the fragile glaze-body bond?

Is the glaze drying too slow?

Is the ware once-fire?

Is the problem happening during firing?

Is there a problem with the body?

Is this problem inherent in the type of glaze being used?

Matte glazes are more prone to crawling. Why? Because they usually have high Al2O3. The major contributor of that oxide is clay, especially kaolin. Matte glazes commonly have 35% kaolin in the recipe. Use part calcined material, part raw kaolin to deal with this problem.

Many pottery glazes have high feldspar and low clay contents, simply because they were improperly formulated. Using chemistry, you can shift the recipe to supply part of the Al2O3 from kaolin instead of the feldspar, reducing the feldspar percentage (this involves corrections in the amount of silica and other materials also).

Slip glazes can have 70, 80 or even 90% of a slip clay in them. Alberta Slip and Ravenscrag slip are examples. These materials melt by themselves to make glazes. But they are clays, they shrink. Follow the instructions from the manufacturer on how to use them properly.

Related Information

Crawling glazes withdraw into islands during melting

The cause is almost always obvious upon seeing the recipe


A glaze is crawling during firing

This picture has its own page with more detail, click here to see it.

This problem is almost always caused by glazes shrinking too much during drying and then cracking. Those cracks become the crawl points during firing. Excessive shrinkage is normally a product of too much raw clay in a glaze. Even glazes a marginally high clay can crack if applied too thickly. It is likewise with multi-layer application done without consideration for the specific needs of that process (e.g. failure to use a base coat glaze for the first layer). Multi-layering of glazes rewets the first layer, stressing its bond with the body and pulling it away from the body as it shrinks. Base coat glazes have better adherence. Crawling is quite prevalent in once-fired ware since glaze bonding is more tenuous. And in zircon opacified glazes.

To state again: Glazes contain clay to suspend their slurries. Clay shrinks when it dries. Some shrinkage can be tolerated but when it is excessive, something has to give. As glaze layer thickness increases, it is afforded more and more power to impose its shrinkage on the bond with the body. At some point, that bond will be compromised in places where cracks occur to release the tension. Even if these do not appear on dry ware, bond compromise can still exist.

ChatGPT is surprisingly wrong about the causes of glaze crawling.


A glaze crawling inside a mug

This picture has its own page with more detail, click here to see it.

ChatGPT trained on the entire internet and yet gave 100% wrong answers and neglected the key thing that causes 90% of crawling! How can the internet be so wrong? Consider the suggestions it gave:

-Dust or oil on the bisque: This almost never happens. Besides, glaze is a mix of dust and water!
-Too much feldspar in a glaze can cause it to shrink excessively during firing: No, high feldspar causes thermal expansion/contraction of the fired glass, not physical shrinkage of the melt.
-If the clay body surface is not roughened, the glaze may not adhere properly: No, glazes don’t crawl any more on porcelains than other bodies.
-If the glaze is too thick in some areas and too thin in others, it can crawl in the thin areas: No, it crawls where thick because that’s where it cracks during drying.
-Over-firing or under-firing: No. Glazes fired to the ideal temperature crawl just as much.
-If the pottery is dried evenly or the drying process is too rapid: No, rapid drying of glaze on bisque is important to prevent cracking.

This crawling happened because the glaze cracked along the inside of that corner during drying. Such cracking is by far the number one cause of crawling, the melt pulls back from either side of the crack. The specific gravity of the slurry was too high, the resulting greater thickness right at the corner gave the shrinking glaze power to pull a crack. Adding water to bring the SG back down to 1.4 and then Epsom salts to gel it to thixotropic gave the slurry much better dipping and drying properties and totally solved this issue.

Clay in a glaze recipe: Why is it there?

What happens when there is too much?


Glaze cracking during drying

This picture has its own page with more detail, click here to see it.

If I put this on social, I might get 100 comments on the cause. Most would say it's applied too thick. That is not correct. At the top, it is too thick, but not at the bottom (where it is still cracking). Crawling during firing is almost certain.

Before offering any opinion, one needs to sanity check the recipe. This one, GA6-B, contains a lot of clay. Why do dipping glazes contain clay, usually kaolin, ball clay? To suspend the slurry, slow down drying, gel the slurry to make it thixotropic and harden the layer on drying. But their chemistry is also important, clays supply the all-important Al2O3 and SiO2 to the melt (which would otherwise have to come from feldspar). Certain clays excel at suspending. 15-20% EP kaolin, for example, is all that is needed. It’s not that plastic, but sticky and thixotropic (Grolleg and New Zealand kaolins are similar or even better). 10% of a gelling ball clay might be enough. However, 50% of a silty non-plastic clay might be needed. When the clay has too much influence, glazes shrink too much as they dry and then crack like this. Ones lacking clay (or employing one that is not suitable) have poor application properties (for dipping) and are powdery. This glaze has 80% pure raw Alberta Slip. That is a plastic clay, no wonder this is happening! 50% of it needs to be roasted.

A thickly-applied dipping glaze has crawled


This picture has its own page with more detail, click here to see it.

Example of cone 6 glaze crawling on the inside of a stoneware mug. The dipping glaze slurry had a high specific gravity (low water content) and built up thickly on the bisque, even with a quick pour. Thickly applied glazes have more ability to assert their shrinkage and thus commonly compromise their bond with the body during drying. The cracks that appear then become bare patches after firing.

Two glazes. One crawls, the other does not. Why?


This picture has its own page with more detail, click here to see it.

The DIY glaze on the right is crawling at the inside corner. Why? Multiple factors contribute.

Majolica glaze crawling on this slip-cast terra cotta


This picture has its own page with more detail, click here to see it.

Mitigating factors are poor adherence of the glaze to the smooth-surfaced L4170B terra cotta bisque, high zircon content in the glaze (it reduces melt fluidity) and the very thick application (this is a variation on G1916Q as a majolica glaze). Which is the most important of those factors? The adherence to the bisque. An addition of Veegum CER solved the problem (50g of the solution to 0.75 litres of glaze slurry, with added water to thin it out). Unlike with CMC gum, this slurry still goes on thick and evenly. Although the piece on the left is darker red, that is a photo issue, these were both the same body and fired at cone 04.

Crawling can happen when paint-on glazes are layered over dipping glazes


The inner glaze has curtained off downward from the rim on buff stoneware bowl

This picture has its own page with more detail, click here to see it.

This bowl was dipped in a non-gummed clear dipping glaze. Such glazes are optimized for fast drying and even coverage. However their bond with the bisque is fragile. The blue over-glaze was applied thickly on the rim (so it would run downward during firing). But during drying, it shrunk and pulled the base coat away at the rim (likely forming many tiny cracks at the interface between the clear and the bisque. That initiated the cascade of crawling. When gummed dipping glazes are going to be painted over, a base-coat dipping glaze should be used. What is that? It is simply a regular fast-dry dipping glaze with some CMC gum added (perhaps half the amount as what would be used for painting). There is a cost to this: Longer drying times after dipping and less even coverage. And gum destroys the ability to gel the glaze and make the slurry thixotropic.

Faux majolica next level: Stoneware!

But the glaze is crawling under the colors.


This picture has its own page with more detail, click here to see it.

The original Italian majolica ware was red earthenware with a thick layer of tin-opacified glaze vibrantly brush-decorated using single-strokes of watery metal oxides. The water-color of ceramics. But tin oxide is no longer affordable. And ceramic stains are better. And no one uses lead glazes. So all majolica-like ware made today is actually “faux (false) majolica”. These test samples take the “faux” to the next level: Stoneware with a zircon-opacified white glaze. But almost all are crawling. If this happens for you ask these questions:

Is the glaze re-wetable? Dipping glaze recipes often are not, especially if they fail sanity check (e.g. are over-clayed or under-clayed).
Base coat dipping glaze better survive the rewetting of a second layer?
Mixing them as a brushing glaze give maximum insurance.

What did they look like when the overcolor dried? Cracks are sure indicator or crawling.
Were you painting pure stain or metal oxide (mixing with water only)? Don’t do that. Water color paint uses gum Arabic, pottery colors need to be in a stain medium (which often has CMC gum).

Crawling in G2934Y Zircopax white glaze: Here are some fixes.


A matte glazed G2934Y mug where the glaze has crawled on the upper handle join

This picture has its own page with more detail, click here to see it.

G2934Y, a variation of the G2934 base, is a good stain matte base glaze but it is not without issues. It has significant clay content in the recipe and high levels of Al2O3 in the chemistry; these make it susceptible to crawling. This base is normally fine as is, but when opacified or certain stains are added (especially at significant percentages) it can crawl. This has 10% Zircopax. Even though the glaze layer thickens at the recess of the handle join, it is still crawling. We also get this on the insides of mugs where the wall and foot meet at a sharp angle. This was initiated because the glaze cracked here during drying. Normally it would heal, but the zircon stiffens the melt, making it less mobile. The easiest solution is to adjust the specific gravity of the glaze to 1.44 and flocculate it to thixotropic; this assures that the application is not too thick. Another measure is to add a little CMC gum (by replacing some of the water with gum solution). Lastly, use a blend of tin oxide and Zircopax, as in the G3926C version of the recipe, to opacify it.

How much Zircon does it take to make a glaze crawl?

For G2934 cone 6 matte glaze: As little as 5%


G2934 matte glaze is crawling

This picture has its own page with more detail, click here to see it.

The Zircon needed to opacify glazes has a side effect: Crawling. Even low percentages can induce this issue when other factors interplay (as is the case here). It often happens at sharp concaves (e.g. inside bottom corners on mugs). But here it is on surfaces disturbed during formation of the spout. This G2934 recipe has good melt fluidity, so that is not the issue. The issue appears related to adherence of the initial laydown. Here are some questions to consider:

This serious glaze crawling problem was solved with a simple addition


This picture has its own page with more detail, click here to see it.

This is G2934Y white (with 10% Zircopax). I initially blamed the zircon for the crawling. But, since the slurry had settled somewhat I was able to remove about 15% of the water and replace it with CMC gum solution. The gum addition was not enough to slow down the drying much but it really improved reduced the problem! This likely means that adherence of the dried layer to the smooth bisque was the issue. This being said, there were still a couple of small spots where it crawled. The ultimate solution thus appears to be discovering the percentage of CMC gum and water needed to get the least loss of drying speed and while achieving integrity of glaze coverage. It is best to add the CMC gum as a powder at mixing time and blender mix the slurry thoroughly to be sure that it fully dissolves (watch for a rheology change on aging, that will demonstrate if mixing was thorough enough).

Alberta Slip crawling because it shrinks too much on drying


This picture has its own page with more detail, click here to see it.

Example of Alberta Slip which has been sprayed on dry ware and single fired. This happened because the slip shrunk during drying creating a network of cracks. These cracks become the crawl-points during firing.

Badly crawled glaze fired at cone 5 reduction


This picture has its own page with more detail, click here to see it.

It was spray applied on the dried bowl (no bisque fire) an was too thick (not to mention under fired). But the main problem was a glaze recipe having too high a clay content. If a glaze has more than about 25% clay, consider a mix of the raw clay and calcined. For example, you can buy calcined kaolin to mix with raw kaolin. Or you can calcine the clay in bowls in your kiln by firing it to about 1200F.

Fixing a crawling problem with Ravenscrag Tenmoku


This picture has its own page with more detail, click here to see it.

Crawling of a cone 10R Ravenscrag Slip iron crystal glaze. The added iron oxide flocculates the slurry raising the water content, increasing the drying shrinkage. To solve this problem you can calcine part of the Ravenscrag Slip, that reduces the shrinkage.

Crawling glaze on slip cast ware is common


This picture has its own page with more detail, click here to see it.

This cone 6 white glaze is crawling on the inside and outside of a thin-walled cast piece. This happened because the thick glaze application took a long time to dry, this extended period, coupled with the ability of the thicker glaze layer to assert its shrinkage, compromised the fragile bond between dried glaze and fairly smooth body. There are several measures that can be taken to solve this problem. The ware could be heated before glazing, the glaze applied thinner, or glazing the inside and outside could be done as separate operations (with a drying period between).

Same body, same glaze, same firing. Why did one crawl?


Crawling glaze on cast ware

This picture has its own page with more detail, click here to see it.

The body: M370. Glaze: G2934Y (with added green stain). Firing: Cone 6 drop-and-hold. Glazing method: dipping (using tongs). Thickness: The same. Surface: Clean on both. The difference: Clay wall thickness. The one on the right was cast much thinner so the glaze took a lot longer to dry. Common pottery glazes contain clays which need to shrink somewhat during drying. The bond with the bisque, although fragile, is normally enough to prevent cracking during drying. But drying needs to occur quickly with glazes containing no gum hardener - that is only possible when the body has enough porosity to absorb all the water quickly. Otherwise, cracks appear - and they become crawls during firing. A complicating factor is that stain and/or zircon additions make an already crawl-susceptible glaze even worse. One or a combination of the following can be done to minimize crawling on even very thin-walled pieces:
-Apply a thinner glaze layer.
-Heat the bisque before dipping.
-Glaze the inside and outside separately (with drying between).
-Deflocculate the glaze to reduce water content.
-Brush or spray on a CMC gummed version in multiple coats.

Crawling sanitary ware glaze sourcing Al2O3 from only feldspar


This picture has its own page with more detail, click here to see it.

The original recipe had a very low clay content, sourcing almost all of its Al2O3 from feldspar instead. Although the glaze slurry was maintained at 1.78 specific gravity (an incredibly high value) and thus would have had very low shrinkage, it did not stick and harden well enough to the ware. Why? Lack of clay content in the glaze. The fix was to source much more of the Al2O3 from kaolin instead of feldspar. The reduction in feldspar shorted the glaze on KNaO and SiO2 so these were sourced from a frit and pure silica instead (the calculations to do this were done in Insight-live.com). The change also provided opportunity to substitute some of the KNaO with lower expansion CaO. This reduced the thermal expansion and reduced crazing issues.

Zircon glazes cover well but they have a problem


This picture has its own page with more detail, click here to see it.

This sanitary ware tank lid was made in China. Notice how thick the white glaze is being applied to cover the iron containing body below. This is a testament to how opaque a zircon opacified glaze can be. Zircon often causes crawling (likely due to a combination of the effects of its fine particle size on drying properties and its tendency to stiffen the melt). Extra measures and constant attention to detail (e.g. glaze thickness, slurry rheology, avoidance of sharp contours on ware) are needed with such glazes.

Crawling glaze on the convex edges of sanitaryware


crawling glaze on sanitaryware

This picture has its own page with more detail, click here to see it.

Sanitaryware glazes are high in zircon, thus a stiff glaze melt is a part of their very nature. That means glaze crawling is a part of their nature! And, preventing it is a major effort by producers. Crawling most commonly happens inside acute contour changes (that thicken the layer), but crawl points can even occur on relatively flat surfaces. However, this time it appears on the outside of an abrupt curve. Factors that can cause crawling can compound on corners. During drying, soluble salts and binders in the clay tend to concentrate at edges and corners - these can affect glaze laydown (especially its thickness and adhesion). The slip casting process favours the concentration of the finest clay particles at the mold face, but corners see the most surface disruption during cleaning and tooling at the leather hard stage (which can expose coarser particles below the surface). Glazes containing clay must shrink somewhat during drying, a corner like this will be the first place a crack appears (and thus a crawl), especially if adhesion is not as good.

Mag carb causes crawling in higher amounts


This picture has its own page with more detail, click here to see it.

Example of two crawling glazes. Both have magnesium carbonate added to make this happen (around 10%). On the left at cone 04 on a terra cotta body, on the right at cone 6 on a porcelain. Magnesium carbonate also mattes glazes.

Why does the glaze on the right crawl?


This picture has its own page with more detail, click here to see it.

This is G2415J Alberta Slip glaze on porcelain at cone 6. Why did the one on the right crawl? Left: thinnest application. Middle: thicker. Right thicker yet and crawling. All of these use a 50:50 calcine:raw mix of Alberta Slip in the recipe. While that appears fine for the two on the left, more calcine is needed to reduce shrinkage for the glaze on the right (perhaps 60:40 calcine:raw). This is a good demonstration of the need to adjust raw clay content for any glaze that tends to crack on drying. The Alberta Slip and Ravenscrag Slip page have information about how to calcine and calculate how much to use to tune the recipe to be perfect.

Does bisque ware need washing for glazing?

These pieces demonstrate why not.


This picture has its own page with more detail, click here to see it.

A light coating of ordinary ceramic dust is made of the same minerals as the ware and glaze itself. During dipping, the incoming water instantly penetrates and incorporates surface dust. Glaze are dust mixed with water! However, washing trades a tiny and often harmless surface contaminant for a more serious problem: partially saturated pores. Bisqueware is a porous ceramic sponge. Its job during dip glazing is to suck water out of the slurry quickly and evenly, leaving behind a stable layer of particles on the surface. If the bisque is damp from washing, the suction is weakened. Of course, there are common-sense exceptions, but compressed air, a soft brush, or a barely damp sponge used sparingly are better cleaning solutions to preserve the essential dryness.

These thin-walled mugs demonstrate: Just pour-glazing the inside has waterlogged them, they must be dried before applying the outside glaze. Imagine if they had been washed also!

Glaze cracking during drying? Wash it off and then do this.


Glaze spider web cracking on drying

This picture has its own page with more detail, click here to see it.

If your pottery glaze is doing on drying then it will crawl during firing. Wash it off, dry the ware. Then check the water content. If the glaze has worked fine in the past then it is likely going on too thick because the specific gravity is too high - just repeat cycles of adding a little water and dip testing (make it thixotropic if needed). But that was not the issue here. Glazes need clay to suspend and harden them, but too much clay means trouble. This was Ravenscrag Slip, a clay, being used pure as a cone 10R glaze. The glaze appeared to go in perfectly and it dried to the touch in ~20 seconds. But shrinkage continues after that, revealing after a couple of minutes. Fixing the issue was a matter of adding some roasted Ravencrag Slip to the bucket. That reduced the shrinkage and therefore the cracking. Any glaze containing excessive kaolin can be fixed the same way (trade some of the raw kaolin for calcined kaolin). Some glazes that contain plenty of clay also have bentonite - a simple fix for these is to simply remove the bentonite.

CMC Gum is magic for multi-layering, even for raw Alberta Slip


A glaze that cracks on drying was fixed

This picture has its own page with more detail, click here to see it.

The glaze on the left is 85% of a calcine:raw Alberta Slip mix (40:60). It was on too thick so it cracked on drying (even if not too thick, if others are layered over it everything will flake off). The center piece has the same recipe but uses 85% pure raw Alberta Slip, yet it sports no cracks. It should be cracked much worse than #1. How is this possible? 1% added CMC Gum (via a gum solution) was added! This is magic, but there is more. It is double-layered! Plus very thick strokes of a commercial brushing glaze have been applied over that. Yet no cracks. CMC is the secret of dipping-glazes for multi-layering. The downside: More patience during dipping, they drip a lot and take much longer to dry.

Here is why Albany Slip was hard to use:

Cracking during drying, crawling during firing


This picture has its own page with more detail, click here to see it.

This glaze is 85% Albany Slip and 20% Ferro Frit 3195. These bisque tiles were dipped in a brushing glaze version of it (just water and powder). The glaze is applied quite thin on the front tile and thicker on the back one. The material gelled slurries and required a lot of water to make them thin enough to use. For assured success, this or any glaze that had a high percentage required mixing the raw Albany Slip with a calcined Albany Slip (which people had to make on their own).

Fixing a crawling problem with a measured CMC addition


A pail of glaze needs CMC gum

This picture has its own page with more detail, click here to see it.

The problem: This dipping glaze is crawling (as shown on the glazed tile). Let's assume I have already checked to make sure the specific gravity is right and the slurry is thixotropic. Because it has settled a little there is an opportunity for plan B: Remove some of the water and replace it with gum solution. Shown here is a precise calculation of the exact water content of the slurry to replace 10% of the water with gum solution. But it is better to take a more conservative and easier approach: Replace one-twentieth of the water with gum solution (too much gum and the glaze will drip excessively and dry too slowly). Rather than be overly precise let's just guess: I have 5000g of slurry that is about 50% water, so that is 2500g of powder, so I need to remove 125g of water and replace it with 125g of Laguna gum solution. A good way is to use a sponge: Wet and wring it out first and then repeat touching it to the water surface and wringing it out into a container to get 125g. A propeller mixer is needed to mix in the added gum solution (it won't just stir in).

This dipping glaze has too much raw clay:

So it cracks as it dries


A high clay glaze is cracking

This picture has its own page with more detail, click here to see it.

This is an example of how a dipping glaze that contains too much plastic clay has been applied too thickly. It shrinks and cracks during drying and is guaranteed to crawl. This is raw Alberta Slip. To solve this problem, you need to tune a mix of raw and roasted clay. Enough raw clay is needed to suspend the slurry and dry it to a hard surface, but enough calcine is needed to keep the shrinkage low enough that this cracking does not happen. Perhaps you have been using a glaze having a high percentage of clay, and this does not happen - the reason is likely that the clay is not highly plastic.

Multilayer crawling


This picture has its own page with more detail, click here to see it.

Oil-spot effects depend on being able to layer glazes. Normally, a black underneath and matte white over top. Using dipping glazes is obviously advantageous for this type of piece; the second dip covers the other half and creates the double layer needed. But dipping glazes contain clay in the recipe (almost always kaolin or ball clay), it satisfies multiple needs: It suspends the slurry, hardens the drying glaze, and supplies critical Al2O3 to the chemistry. The upper glaze here is a matte; so it needs extra Al2O3, which means it likely has extra clay. 20% kaolin (non-plastic like EPK, Grolleg, NZ) is about the maximum or the glaze will shrink too much when drying. If extra Gerstley Borate is added, then it will be worse. Drying cracks are the result when the fragile body-bond of the lower one fails to withstand the stresses of being rewetted and tugged upon by the upper layer being applied and drying. When the cracked double-layer begins to melt, it pulls itself into islands, leaving bare body between. That is called "crawling".

How to prevent this. Be smart about glaze layering and use recipe logic. The lower black can likely be adjusted to be a first coat dipping glaze. The clay content in the upper white one can be adjusted to reduce drying shrinkage (by splitting it between raw and roasted/calcined powder, or by using a clay having lower plasticity).

Links

Articles Understanding Glaze Slurry Properties
It is possible to have a glaze slurry that is a joy to use, but only if you understand the physics of the materials in the glaze recipe.
Articles Creating a Non-Glaze Ceramic Slip or Engobe
It can be difficult to find an engobe that is drying and firing compatible with your body. It is better to understand, formulate and tune your own slip to your own body, glaze and process.
Materials Calcined Kaolin
This is kaolin powder that has been fired in a furnace to remove the 12% crystal water and render it non-plastic.
Materials Alberta Slip 1000F Roasted
Materials Light Magnesium Carbonate
A refractory feather-light white powder used as a source of MgO and matting agent in ceramic glazes
Materials Alberta Slip 1900F Calcined
Materials Ravenscrag Slip
A light-colored silty clay that melts to a clear glaze at cone 10R, with a frit addition it creates a good base for a wide range of cone 6 glazes.
Materials Alberta Slip
Albany Slip successor - a plastic clay that melts to dark brown glossy at cone 10R, with a frit addition it can also host a wide range of glazes at cone 6.
Glossary Glaze Layering
In hobby ceramics and pottery it is common to layer glazes for visual effects. Using brush-on glazes it is easy. But how to do it with dipping glazes? Or apply brush-ons on to dipped base coats?
Glossary Ceramic Glaze Defects
Ceramic glaze defects include things like pinholes, blisters, crazing, shivering, leaching, crawling, cutlery marking, clouding and color problems.
Glossary Surface Tension
In ceramics, surface tension is discussed in two contexts: The glaze melt and the glaze suspension. In both, the quality of the glaze surface is impacted.
Glossary Glaze Crawling
A ceramic glaze fault that occurs during firing of the ware, the molten glaze pulls itself into islands leaving bare patches of body between.
Glossary Suspension
In ceramics, glazes are slurries. They consist of water and undissolved powders kept in suspension by clay particles. You have much more control over the properties than you might think.
Glossary Calcination
Calcining is simply firing a ceramic material to create a powder of new physical properties. Often it is done to kill the plasticity or burn away the hydrates, carbonates, sulfates of a clay or refractory material.
Oxides Sm2O3 -
Troubles Glaze Pinholes, Pitting
Analyze the causes of ceramic glaze pinholing and pitting so your fix is dealing with the real issues, not a symptom.
Troubles Glaze peeling on drying
Happens as clay-containing glazes shrink during drying on the bisque ware, first cracking then pulling away.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy