Ag2O | AlF3 | As2O3 | As4O6 | Au2O3 | BaF2 | BeO | Bi2O3 | CaF2 | CdO | CeO2 | Cl | CO | CrO3 | Cs2O | CuCO3 | Dy2O3 | Er2O3 | Eu2O3 | F | Fr2O | Free SiO2 | Ga2O3 | GdO3 | GeO2 | HfO2 | HgO | Ho2O3 | In2O3 | IrO2 | KF | KNaO | La2O3 | Lu2O3 | Mn2O3 | MoO3 | N2O5 | NaF | Nb2O5 | Nd2O3 | Ni2O3 | OsO2 | Pa2O5 | PbF2 | PdO | PmO3 | PO4 | Pr2O3 | PrO2 | PtO2 | RaO | Rb2O | Re2O7 | RhO3 | RuO2 | Sb2O3 | Sb2O5 | Sc2O3 | Se | SeO2 | Sm2O3 | Ta2O5 | Tb2O3 | Tc2O7 | ThO2 | Tl2O | Tm2O3 | Trace | U3O8 | UO2 | WO3 | Y2O3 | Yb2O3

CaO (Calcium Oxide, Calcia)

Data

Co-efficient of Linear Expansion 0.148
Frit Softening Point 2910C (From The Oxide Handbook We also have a figure of 2572?)

Notes

CaO is not found pure in nature but rather is contained in various abundant minerals (i.e. calcite, aragonite, limestone, marble), but vary greatly in their purity (impurities usually include magnesia, iron, alumina, silica, sulfur). Of these iron and sulfur are most troublesome (i.e. where clarity is important in glass). Lime minerals vary in the degree of crystallization and cohesion of the crystalline mass and the homogeneity of the matrix.

-Together with SrO, BaO, and MgO it is considered one of the Alkaline Earth group of oxides. It has a cubic crystal structure.

-Quicklime is pure calcia, but it reacts with water to produce calcium hydroxide or slaked lime. Calcium oxide, on the other hand, is an extremely stable compound.

-Calcia alone resists melting even at very high temperatures (an incredible 2600C). It can be smelted with Al2O3 to produce refractory calcium aluminate cement (which can service to 2000C). But when soda and potash are added, CaO becomes a very active flux in both oxidation and reduction. This synergy between CaO and other fluxes and differences in the mechanism of its fluxing action generates some disagreement among experts regarding the nature of CaO (like MgO, it is not a 'stand-alone' flux).

-At higher temperatures, CaO contributed by wollastonite is more readily fusible than that contributed by whiting (calcium carbonate). Stain manufacturers recommend adding the molecular equivalent of calcium oxide using wollastonite, for better uniformity.

-Calcium oxide is the principal flux in medium and high temperature glazes, beginning its action (within the glaze) around 1100C. It must be used with care in high-fire bodies because its active fluxing action can produce a body that is too volatile (melting if slightly overfired).

-Calcia usually hardens a glaze and makes it more scratch and acid-resistant. This is especially so in alkaline and lead glazes. However the increased hardness does not necessarily mean greater tensile strength. Its thermal expansion is intermediate.

-CaO is not effective below cone 4 as a flux in glazes but in small amounts (less than 10%) it can dissolve in earthenware glaze melts, especially with lead, soda, potash) to add hardness and resistance to leaching. In non-lead mixes it can also help reduce crazing. In larger amounts, it encourages the growth of crystals which can give decorative effects to glossy glazes and produce matteness (i.e. 30%).

-High CaO glazes tend to devitrify (crystallize). This occurs either because of the high melt fluidity imparted by CaO at higher temperatures or because of the readiness with which CaO forms crystals. Fastfire glazes can contain more CaO because the quick cooling does not give the crystallization a chance to occur.

-Calcia is a moderate flux in the cone 5-6 range, but a very active one at cone 10.

-High calcia glazes tend to have good (although sometimes unexpected) color responses. For example, in oxidation iron glazes calcia likes to form yellow crystalline compounds with the Fe2O3, producing a 'lime matte'. Without the calcia, glossy brown glazes are the norm. CaO can bleach or soften colors, especially with cobalt (pastel tones). That being said, CaO is relatively neutral with most pigments, not pushing or pulling color hues strongly.

The term 'lime' encompasses several different minerals and manufactured products.

-The term 'Whiting' traditionally refers to calcium carbonate produced by the grinding of chalk from the cliffs of England, Belgium and France. However this title also refers to any ground calcium carbonate material (i.e. those processed from marble and calcite ores).

-Ground limestone and calcined limestone (burned lime) are used in the glass industry. Float and container glass have 10% CaO.

-Dolomite (magnesium carbonate) is a mineral which supplies some magnesia in addition to its CaO complement. It is preferred in many situations because it more readily fluxes and the magnesia imparts desirable properties.

-Wollastonite is a calcium silicate which is more expensive than other sources of calcium, but is used bodies, glaze, porcelains, enamels and frits for its many superior properties.

Stull chart showing the SiO2-Al2O3-(0.7CaO+0.3KNaO) system


This picture has its own page with more detail, click here to see it.

The original Stull chart - Chart 1 from Transactions of the American Ceramic Society, Vol. XIV (1912). Stull mapped test glazes by their SiO2:Al2O3 molar ratio and identified the regions that predict surface quality.

If you really want to "get into the weeds" of glaze chemistry, the https://stullatlas.app tool, by Ryan Lack, takes Stull's insight and applies it to a modern dataset of real-world glazes, giving you an interactive map of the glaze chemistry landscape. The primary dataset comes from Glazy. It contains thousands of community-contributed recipes with calculated UMF values, cone temperatures, surface types, and firing atmospheres. Each point on the chart represents a real glaze recipe that someone has mixed, fired, and documented.

Phase diagram of a SiO2:Al2O3:CaO:KNaO System


This picture has its own page with more detail, click here to see it.

Phase diagram and stull chart showing the SiO2-Al2O3-(0.7CaO+0.3KNaO) system.
Courtesy of Matthew Katz, Alfred University

Two stains. 4 colors. Will the guilty oxide please step forward.


One stain produces clear in one glaze and red in another. Another stain blue and purple. Why?

This picture has its own page with more detail, click here to see it.

These pairs are G2934 matte and G2916F glossy cone 6 base glaze recipes. The left pair has 5% maroon stain added, the right pair 5% purple stain. Why? The Mason Colorworks reference guide has the same precaution for both stains: the host glaze must be zincless and have 6.7-8.4% CaO (this is a little unclear, it is actually expressing a minimum, the more the CaO the better). The matte recipe calculates to 11% CaO, the glossy to 9%. So there is enough CaO. The problem is MgO (it is the mechanism of the matteness in the left two), it impedes the development of both colors (although not mentioned on the Mason docs).

Ceramic Oxide Periodic Table

Periodic table of ceramic oxides

Pretty well all common traditional ceramic base glazes are made from less than a dozen elements (plus oxygen). Go to the full picture of this table and click or tap each of the oxides to learn more (on its page at digitalfire.com). When materials melt, they decompose, sourcing these elements in oxide form. The kiln builds the glaze from them, it does not care what material sources what oxide (assuming, of course, that all materials do melt or dissolve completely into the melt to release those oxides). Each of these oxides contributes specific properties to the glass. So, you can look at a formula and make a good prediction of the properties of the fired glaze. And know what specific oxide to increase or decrease to move a property in a given direction (e.g. melting behavior, hardness, durability, thermal expansion, color, gloss, crystallization). And know about how they interact (affecting each other). This is powerful. A lot of ceramic materials are available, hundreds - that is complicated when individual materials source multiple oxides. Viewing a glaze as a simple unity formula of ceramic oxides is just simpler.

Boron blue in low-fire transparent glazes


This picture has its own page with more detail, click here to see it.

This high-boron high-CaOcone 04 glaze is generating calcium-borate crystals during cool-down (called boron-blue). This is a common problem and a reason to control the boron levels in transparent glazes; use just enough to melt it well. If more melt fluidity is needed, decrease the percentage of CaO in favor of a lower-melting oxide, that will certainly help. There is a positive: For opaque glazes, this effect can actually enable the use of less opacifier (among the most expensive of all materials).

Glaze chemistry works best when changing material amounts, not material types


This picture has its own page with more detail, click here to see it.

Two glazes, same chemistry, different materials. The glaze on the left is sourcing CaO from wollastonite, the one on the right from calcium carbonate. Thus the oxide chemistry of the two is the same but the recipe of materials sourcing that chemistry is different. The difference in this GLFL test for melt flow is an expression of how choosing different mineral sources to source an oxide can produce melting patterns that go outside what the chemistry suggests. The difference here is not extreme, but it can be much more.

The difference between dolomite and calcium carbonate in a glaze


This picture has its own page with more detail, click here to see it.

These glaze cones are fired at cone 6 (without slow cooling) and have the same recipe: 20 Frit 3134, 21 EP Kaolin, 27 calcium carbonate, 32 silica. The difference: The one on the left uses dolomite instead of calcium carbonate. Notice how the MgO from the dolomite mattes the surface (without slow cooling) whereas the CaO from the calcium carbonate produces a brilliant gloss (because it needs slow cooling).

Add 5% calcium carbonate to a tenmoku. What happens?


This picture has its own page with more detail, click here to see it.

In the glaze on the left (90% Ravenscrag Slip and 10% iron oxide) the iron is saturating the melt crystallizing out during cooling. GR10-K1, on the right, is the same glaze but with 5% added calcium carbonate. This addition is enough to keep most of the iron in solution through cooling, so it contributes to the super-gloss deep tenmoku effect instead of precipitating out.

Comparing two glazes having different mechanisms for their matteness


This picture has its own page with more detail, click here to see it.

These are two cone 6 matte glazes (shown side by side in an account at Insight-live). G1214Z is a calcia matte, it has a high silica:alumina ratio. It crystallizes during cooling to make the matte effect. Melt fluidity is needed for that and this GLFL test shows that it certainly has that. The degree of matteness is adjustable by tuning the SiO2 content. The G2928C is a magnesia matte, it has high MgO and produces the classic silky micro-wrinkled the surface. Its matteness is adjustable by trimming the calcined kaolin. CaO is a standard oxide that is in almost all glazes, 0.4 is not high for it. But much less MgO is needed for it to make a matte. The G2928C also has 5% tin, if that was not there it would be darker than the other one because Ravenscrag Slip has some iron. This glaze actually has texture like a dolomite matte at cone 10R, it is great. And it has wonderful application properties. And it does not craze, on Plainsman M370 (it even survived a 300F-to-ice water IWCT test). This looks like it could be a great liner glaze.

CaO is a strong flux but it can cause crazing


This picture has its own page with more detail, click here to see it.

2, 5, 10, 15% calcium carbonate added to Ravenscrag Slip on a buff stoneware fired at cone 10R. It gets progressively glossier toward 15%, crazing starts at 10% (test by Kat Valenzuela). Adding a flux only reduces the SiO2 and Al2O3, this pushes the thermal expansion upwards. 5% is actually sufficient. An alternative would be to use wollastonite, it supplies SiO2 also.

Links

Materials Wollastonite
Materials Calcium Carbonate
In ceramics, calcium carbonate is primarily a source of CaO in raw stoneware and porcelain glazes.
Materials Calcium Feldspar
Materials Colemanite
A natural source of boron that melts at a very low temperature.
Materials Dolomite
An inexpensive source of MgO and CaO for ceramic glazes, also a highly refractory material when fired in the absence of reactant fluxes.
Materials Quicklime
Materials Calcium Aluminate Cement
Glossary Ceramic Oxide
In glaze chemistry, the oxide is the basic unit of formulas and analyses. Knowledge of what materials supply an oxide and of how it affects the fired glass or glaze is a key to control.
Glossary Limit Formula
A way of establishing guideline for each oxide in the chemistry for different ceramic glaze types. Understanding the roles of each oxide and the limits of this approach are a key to effectively using these guidelines.
Glossary Flux
Fluxes are the reason we can fire clay bodies and glazes in common kilns, they make glazes melt and bodies vitrify at lower temperatures.
Glossary Alkaline Earths
Refers to a group of ceramic fluxing oxides that contribute similar properties to fired glazes. They contrast with the alkalis which are stronger fluxes.
Glossary Oxide Interaction
In ceramic glazes each oxide generally makes a specific contributions to the melting and freezing behavior of the glaze. However interactions are also important.
Oxides MgO - Magnesium Oxide, Magnesia
Minerals Limestone
Limestone forms by sedimentation, of coral and shells (biological limestone) or by the precipitation
Minerals Dolomite
Dolomite, as a rock, is called "dolomitic limestone". It is a carbonate, similar to limestone, but h
URLs http://en.wikipedia.org/wiki/CaO
Calcium Oxide on Wikipedia

Mechanisms

Glaze ColorIn oxidation, iron glazes calcia likes to form yellow crystalline compounds with the Fe2O3 producing a 'lime matte' even in an otherwise fluid glaze.
Glaze ColorCalcia likes to form yellow crystalline compounds with Fe2O3 producing a 'lime matte', especially in fluid glazes. Thus iron glossy brown or black glazes should be low in CaO.
Glaze MattenessHigh molar amounts of calcia combined with adequate silica and preferably lower alumina will form a calcium silicate crystal matte (lime matte). The presence of zinc will increase the size of crystals.
Glaze VariegationCaO can mottle glaze surfaces at high temperatures if significant amounts are present, it is a very strong flux and can contribute to phase separation.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy