Being able to mix your own clay body and glaze from native materials might seem ridiculous, yet Covid-19 taught us about the need for independence.
Would you like to be more independent? Understand your clay body? Employ native materials body recipes? Be able to adjust and improve them? Even formulate bodies from scratch? The first step is to find a clay in your area. Read the article (link below) on how to find and test your own native materials. Consider some of the possibilities of what you might find:
-A best-case scenario is that you find pentunse in China, a "Mother Natures porcelain". Just add kaolin and bentonite. PV Clay from California is a similar story. Also 3B clay from Plainsman Clays.
-What might appear to be a worst-case scenario is that you find a fireclay. What good would that be for pottery? Fireclays are often just the crude form of ball clays. Slurry and screen and add about 30% feldspar and you have a cone 6 stoneware. A super plastic one.
-If your clay is extremely sticky and takes a long time to dry it could be bentonitic. That means that it is best used as an additive to other clays that are less workable, to impart plasticity. Bodies made having a high percentage of bentonite can be thrown incredibly thin on the potter's wheel. But they must be dried very slowly to avoid cracking.
-If your clay is dark-colored (brown or red) then it could be a middle temperature stoneware (as demonstrated in your initial firing tests as described in the already-referenced article). Plainsman M2 is such a material. These clays are among the most sought after by stoneware potters for the beautiful natural-looking surfaces they can produce around 2200F. Because iron (which produces the brown color) is also a flux, these types of clays rarely have a firing curve the extends to cone 10.
-Dark colored clays can also be terra cotta clays. Terra cottas are also often shades of green and yellow. This demonstrates the amazing number of forms in which the iron oxide in the clays can exist, each having its own color. Terra cotta clays have a short firing range, but with modern kilns that is not a problem. Every clay has an optimal firing range at which it produces the most dense and strong fired product, terra cotta is no different. While the point of maximum density for mid and high temperature materials often never finds zero porosity, terra cotta materials often do. That is the density of glass, creating amazingly strong ware. Actually, firing shy of that, permitting some porosity, can produce beautiful red color and also very good strength. It can be rewarding and a real adventure, finding successful glazes and processes for this type of material.
-If your clay is grey or buff or even white, you may found a buff burning stoneware. These are common in nature, and obviously very useful. If they are not quite vitreous enough, a little talc (1-2%) may be all that is needed. Failing that, some feldspar should make them vitrify at cone 6. At cone 10 they could work all by themselves (Plainsman A3 is an example).
-You may be lucky enough to find a kaolin. White, not very plastic, incredibly smooth. But having plenty of gravel and sand and mineral particle impurities. These clays may not look promising at first, but try to see them for what they could be if you screen out the impurities.
-If your clay is grey, even dark grey, you likely have a ball clay. Treat it like the fireclay mentioned above. That being said, some ball clays can be quite white in color. They are a very special find, gifting plasticity and fired whiteness in the same package. Typically they just need a non-plastic filler. Since ball clays are refractory, you need to add feldspar anyway, so that does double duty as the filler and plasticity cutter. It is also likely that some quartz will be needed for glaze fit, that will further cut the plasticity and bring it into the range of what a throwing body should be.
In any of the clays above you may encounter soluble salts that cause efflorescence (an unsightly scum on the fired surface, see the article referenced below for more info).
With all of these clays you will need to slurry and dewater them for use (unless you have a clay mixer). The advantage of slurrying is that it presents the option of wet-screening to remove impurities.

This picture has its own page with more detail, click here to see it.
These are small-scale devices that work on the same principles as industrial ones - thus they put industrial methods of clay processing in the hands of a potter or hobbyist. These products are stainless steel and food grade and most can be used with powders or shurries and have interchangeable screens. The most expensive device here costs $5000 and the least expensive is far less than $1000. The suppliers of each of these also have other similar machines (as well as other types of processing equipment potentially valuable in small-scale ceramic production).

This picture has its own page with more detail, click here to see it.
This post got a lot of negative reaction on social media. To be clear, I work both sides of the fence, making my living on selling prepared glazes and clay bodies but I get my satisfaction being closer to the materials and processes. That is what enables me to give customer support. I am not an artist, ceramic art is outside the scope of this page. For part of my life in the craft of pottery I am also guilty of what I lament below. In all my years dealing with customer traffic at our store I have never once had a customer that was offended by seeing new clay and glaze recipes we are discovering in the studio and lab, that are better and cheaper than prepared ones. But online some are somehow offended by what follows. 80 manufacturers are selling convenience and encouraging disconnection - although I work for one of them I am a voice of caution about this.
This book was once a “Bible” of hobby and professional potters. They were independent and resourceful. They made their own clays and glazes, knew the materials, built their own kilns. Now we scan social media sites for ideas on layering expensive prepared goopy brushing glazes and hope they melt together into something presentable. Many have even forgotten how to wedge clay properly. We describe processes using mystical art language and exchange likes and poor advice on social media. Those who still know how to retotal a recipe and venture into mixing their own often end up in the online trafficking of an endless parade of recipes that don’t work. Now we even outsource design to AI. Even Nigeria, the very country about whom Cardew wrote, has lost its pottery tradition.
I never appreciated the book back there. Even though he came to visit us in 1973. I have always just taken whatever clay I needed out of our warehouse, but now that I very often make my own clay it really resonates. I got this copy on eBay, I value it as an inspiration to be more closely connected with the planet and the minerals it gifts us (of course I would not do everything as he does). He was no dinosaur, he understood and taught glaze chemistry and material mineralogy, his work was the basis for many prepared glazes we buy today. "Progress" is defined by some as convenience products that make modern ceramics easy. But I believe that, for many, progress is arming yourself with a little more understanding - it enables making better quality ware, in less time, for less expense and time than with prepared products.

This picture has its own page with more detail, click here to see it.
This is an extreme example of firing a clay at many temperatures to get a wide-angle view of it. These SHAB test bars characterize a terra cotta body, L4170B. While it has a wide firing range, its "practical firing window" is much narrower than these fired bars and the graph suggest. On paper, cone 5 hits zero porosity. And, in hand, the bar feels like a porcelain. But ware warps during firing, and transparent glazes will be completely clouded with bubbles (when pieces are glazed inside and out). What about cone 3? Its numbers put it in stoneware territory, watertight. But decomposition gases still bubble glazes! Cone 2? Much better; it has below 4% porosity (any fitted glaze will make it watertight), below 6% fired shrinkage, still very strong. But there are still issues: Accidental overfiring drastically darkens the color. Low-fire commercial glazes may not work at cone 2. How about cone 02? This is a sweet spot. This body has only 6% porosity (compared to the 11% of cone 04). Most low-fire cone 06-04 glazes are still fine at cone 02. And glaze bubble-clouding is minimal. What if you must fire this at cone 04? Pieces will be "sponges" with 11% porosity, shrinking only 2% (for low density, poor strength). There is another advantage of firing as high as possible: Glazes and engobes bond better. An example of a low-fire transparent base that works fine on this up to cone 2 is G1916Q.

This picture has its own page with more detail, click here to see it.
We tested four different clays (brought in by customers). One is from BC and three from Alberta. These fired sample bars show rich color, low soluble salts and high density and strength at very low temperatures. L4233 (left): Cone 06 to 3 (bottom to top). Reaches stoneware-density at cone 02 (middle bar). Plasticity is very low (drying shrinkage is only 4.5%). But, it is stable even if over-fired. L4254 (center bottom): Cone 04,02,3,4 (bottom to top). Very fine particled but contains an organic that is gassing and bloating the middle two bars. L4243: Fires lighter and looks stable here (cone 02,01,1,2 shown) but melts suddenly less than a cone above the top bar (well before vitrification is reached). L4242 (right): Hyper-plastic, with 12% drying shrinkage! Already melting by cone 02 (third from top). Achieves almost zero porosity (porcelain density) at cone 04 (#2 bar). Even when mixed with 20% kaolin and 20% silica it still hits zero porosity by cone 1. What next? I'll mix L4233 (left) and L4242 (right), that should produce stoneware density at cone 02 (about 1% porosity).

This picture has its own page with more detail, click here to see it.
These are raw clays behind the Plainsman Clays plant. The top one is a middle temperature stoneware. All it needs is a little bentonite (about 2-3%) to be a plastic, smooth, vitreous throwing body. If it was not mature at cone 6, that would be easy to fix by the addition of a little feldspar. Any fired-speck-producing impurities can be removed by using a propeller mixer to slurry it and then putting it through a screen (e.g. 60 mesh). After dewatering on a plaster table I am ready-to-go. And that bottom pile? That is the main ingredient in Ravenscrag Slip. All it needs is some feldspar and frit to be a base glaze at cone 6. It is non-plastic and easy to screen (although not really needed since it has few particulate impurities). Likely there are clays in your area you could use to make your own clay bodies and glazes also. The key is to characterize the material first so you know what type of body it would be best for and what to add to get it there.

This picture has its own page with more detail, click here to see it.
Left: 65% #6Tile kaolin and 35% nepheline syenite. Although it has great plasticity and fires white, it crazes the glaze and has 1% fired porosity (using the SHAB test).
Right: 65% M23 Old Hickory ball clay (similar to OM#4) and 35% nepheline syenite (feldspar would also work). The glaze fits, the body fires very dense (zero porosity) and plasticity is fantastic!
The body on the left needs a 20% silica addition (to stop the crazing) and more nepheline (to reduce porosity to porcelain levels). The remaining 40% kaolin will not be nearly enough for a workable plasticity (so bentonite will be needed). The body on the right does not need fixing; it works as is. Many feel that stoneware body recipes must be built on a feldspar-containing base clay having pottery plasticity (adding ball clay, kaolin, feldspar and silica and ending up with needlessly complicated recipes). But, ball clay is a base, all it needs is a non-plastic filler (to cut plasticity and therefore drying shrinkage) and a flux to vitrify it - feldspar or nepheline fills both roles.
Of course, this stoneware does not fire as white. But do you need white? Glazes will fire brightly colored on this surface. And, cleaner ball clays are available in many areas (even ball clays intended for casting will be plastic enough). It is also worth considering the use of a white engobe.

This picture has its own page with more detail, click here to see it.
Consider the advantages of making your own clay bodies using a propeller mixer and plaster table.
-Independence: You control product availability, quality and consistency.
-Flexibility: You control the recipe (with our help if needed). Fine-tune and adjust it over time to fit your needs and compensate for variations in material properties and supply.
-Special-purpose clay bodies are possible, ones that ceramic suppliers do not or cannot make.
-The slurry up process achieves better mixing and deairing than any pugmill. No aging needed.
-A mixer and plaster table are useful for so many other things in a pottery studio.
-Achieving the right stiffness is an integral part of the process.
-Recycling scrap, by slaking, fits the process.
-Local native clays: Slurries enable the use of a magnet to remove iron, a sieve to remove particulates and a settling process to remove soluble salts.
-Cleanup is easy so many kinds of clay can be made without cross contamination.
-It is rewarding - you will own the whole process, the bragging rights alone make it worthwhile for me!
| Glossary |
Characterization
In ceramics, this normally refers to the process of doing physical or chemical testing on a raw material to accurately describe it in terms of similar ones. |
| Glossary |
Brick Making
Brick-making is surprisingly demanding. Materials blending and processing, forming, drying and firing heavy and thick objects as fast as possible are like no other ceramic manufacturing challenge. |
| Glossary |
Clay body
A term used by potters and in the ceramic industry. It refers to the earthenware, stoneware or porcelain that forms the piece (as opposed to the engobe and covering glaze). |
| Glossary |
Soluble Salts
In ceramics, certain compounds in clays and glazes can dissolve into the water, then on drying these are left on the surface. |
| Glossary |
Plaster table
Essential in a pottery studio for dewatering reclaim clay, stiffening clay that is too soft or making your own clay bodies. |
| Glossary |
Propeller Mixer
In ceramic studios, labs and classrooms, a good propeller mixer is essential for mixing glaze and body slurries. |
| URLs |
https://insight-live.com/insight/help/It+Starts+With+a+Lump+of+Clay-433.html
Case Study: Testing a Native Clay Using Insight-Live.com |
| Projects |
Slurry Mixing and Dewatering Your Own Clay Body
Weigh out the ingredients, mix them using your propeller mixer and then dewater and fine-tune the stiffness on your plaster table. |
| Articles |
How to Find and Test Your Own Native Clays
Some of the key tests needed to really understand what a clay is and what it can be used for can be done with inexpensive equipment and simple procedures. These practical tests can give you a better picture than a data sheet full of numbers. |
| Tests |
Shrinkage/Absorption Test
SHAB Shrinkage and absorption test procedure for plastic clay bodies and materials |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk