A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025A Low Cost Tester of Glaze Melt FluidityA One-speed Lab or Studio Slurry MixerA Textbook Cone 6 Matte Glaze With ProblemsAdjusting Glaze Expansion by Calculation to Solve ShiveringAlberta Slip, 20 Years of Substitution for Albany SlipAn Overview of Ceramic StainsAre You in Control of Your Production Process?Are Your Glazes Food Safe or are They Leachable?Attack on Glass: Corrosion Attack MechanismsBall Milling Glazes, Bodies, EngobesBinders for Ceramic BodiesBringing Out the Big Guns in Craze Control: MgO (G1215U)Can We Help You Fix a Specific Problem?Ceramic Glazes TodayCeramic Material NomenclatureCeramic Tile Clay Body FormulationChanging Our View of GlazesChemistry vs. Matrix Blending to Create Glazes from Native MaterialsConcentrate on One Good GlazeCopper Red GlazesCrazing and Bacteria: Is There a Hazard?Crazing in Stoneware Glazes: Treating the Causes, Not the SymptomsCreating a Non-Glaze Ceramic Slip or EngobeCreating Your Own Budget GlazeCrystal Glazes: Understanding the Process and MaterialsDeflocculants: A Detailed OverviewDemonstrating Glaze Fit Issues to StudentsDiagnosing a Casting Problem at a Sanitaryware PlantDrying Ceramics Without CracksDuplicating Albany SlipDuplicating AP Green FireclayElectric Hobby Kilns: What You Need to KnowFighting the Glaze DragonFiring Clay Test BarsFiring: What Happens to Ceramic Ware in a Firing KilnFirst You See It Then You Don't: Raku Glaze StabilityFixing a glaze that does not stay in suspensionFormulating a body using clays native to your areaFormulating a Clear Glaze Compatible with Chrome-Tin StainsFormulating a PorcelainFormulating Ash and Native-Material GlazesG1214M Cone 5-7 20x5 glossy transparent glazeG1214W Cone 6 transparent glazeG1214Z Cone 6 matte glazeG1916M Cone 06-04 transparent glazeGetting the Glaze Color You Want: Working With StainsGlaze and Body Pigments and Stains in the Ceramic Tile IndustryGlaze Chemistry Basics - Formula, Analysis, Mole%, UnityGlaze chemistry using a frit of approximate analysisGlaze Recipes: Formulate and Make Your Own InsteadGlaze Types, Formulation and Application in the Tile IndustryHaving Your Glaze Tested for Toxic Metal ReleaseHigh Gloss GlazesHire Us for a 3D Printing ProjectHow a Material Chemical Analysis is DoneHow desktop INSIGHT Deals With Unity, LOI and Formula WeightHow to Find and Test Your Own Native ClaysI have always done it this way!Inkjet Decoration of Ceramic TilesIs Your Fired Ware Safe?Leaching Cone 6 Glaze Case StudyLimit Formulas and Target FormulasLow Budget Testing of Ceramic GlazesMake Your Own Ball Mill StandMaking Glaze Testing ConesMonoporosa or Single Fired Wall TilesOrganic Matter in Clays: Detailed OverviewOutdoor Weather Resistant CeramicsPainting Glazes Rather Than Dipping or SprayingParticle Size Distribution of Ceramic PowdersPorcelain Tile, Vitrified TileRationalizing Conflicting Opinions About PlasticityRavenscrag Slip is BornRecylcing Scrap ClayReducing the Firing Temperature of a Glaze From Cone 10 to 6Setting up a Clay Testing Program in Your Company or StudioSimple Physical Testing of ClaysSingle Fire GlazingSoluble Salts in Minerals: Detailed OverviewSome Keys to Dealing With Firing CracksStoneware Casting Body RecipesSubstituting Cornwall StoneSuper-Refined Terra SigillataThe Chemistry, Physics and Manufacturing of Glaze FritsThe Effect of Glaze Fit on Fired Ware StrengthThe Four Levels on Which to View Ceramic GlazesThe Majolica Earthenware ProcessThe Potter's PrayerThe Right Chemistry for a Cone 6 Magnesia MatteThe Trials of Being the Only Technical Person in the ClubThe Whining Stops Here: A Realistic Look at Clay BodiesThose Unlabelled Bags and BucketsTiles and Mosaics for PottersToxicity of Firebricks Used in OvensTrafficking in Glaze RecipesUnderstanding Ceramic MaterialsUnderstanding Ceramic OxidesUnderstanding Glaze Slurry PropertiesUnderstanding the Deflocculation Process in Slip CastingUnderstanding the Terra Cotta Slip Casting Recipes In North AmericaUnderstanding Thermal Expansion in Ceramic GlazesUnwanted Crystallization in a Cone 6 GlazeUsing Dextrin, Glycerine and CMC Gum togetherVolcanic AshWhat Determines a Glaze's Firing Temperature?What is a Mole, Checking Out the MoleWhat is the Glaze Dragon?Where do I start in understanding glazes?Why Textbook Glazes Are So DifficultWorking with children
Glaze chemistry using a frit of approximate analysis
Description
Many of the best frits do have a published chemistry, or the chemistry is approximate. Can we still use them in glaze chemistry? Yes.
Article
Is this possible? Yes. How? Relativity is the key. Consider thermal expansion. Rather than try to predict absolute thermal expansions for specific chemistry profiles, it is more practical to try move the chemistry of a glaze in a specific direction to adjust the fired expansion. For example, a crazing glaze needs to have the thermal expansion reduced to reduce the crazing. A cycle of calculations and then physical testing will achieve the desired goal.
An effective strategy to stop crazing is to reduce the amount of KNaO in a recipe and substitute fluxing oxides of lower thermal expansion (like MgO, Li2O, CaO, Sro). Suppose a recipe contains a frit of approximate chemistry (where the frit company releases a chemistry that shows a range for each of the oxides rather than exact amounts) also contains significant feldspar and silica. Without touching the frit, we are in a position to reduce the feldspar and introduce materials that source the desired fluxing oxide(s) (and then add or remove clay and silica to rebalance the SiO2 and Al2O3 amounts). Even if the mystery frit contains KNaO it does not matter, its contribution will be constant, we are adjusting with other materials that also supply it. But there are a guideline or two to follow to make success more likely:
-You must maintain the same total for the recipe and the mystery frit amount also must remain unchanged.
-Compensate when adjusting material amounts where a significant LOI is involved. For example, whiting has a 50% loss on firing. That would mean that for every 1% calcium carbonate lost the recipe total drops by 0.5%. Watch the LOI that Insight calculates, keep the total minus the LOI the same as the original. For example, if the original glaze has a 10% LOI that means you only actually have 90% that goes into making the fired glaze. If you make changes that produce a recipe having a 95% LOI, the recipe total is now greater and the frit is proportionately less.
-In your calculations, use an average of the oxide ranges given for the frit as if it were the actual chemistry, this enables you to make better decisions about the most appropriate kinds of changes you could make to the chemistry to achieve the desired goal. Often the amount of the frit may be less than 30% and thus the calculation of the final chemistry of the glaze is not altogether inaccurate.
 PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
|
By Tony Hansen Follow me on
 |  |
Got a Question?
Buy me a coffee and we can talk 
https://backup.digitalfire.com, All Rights Reserved
Privacy Policy