All Articles
A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025A Low Cost Tester of Glaze Melt FluidityA One-speed Lab or Studio Slurry MixerA Textbook Cone 6 Matte Glaze With ProblemsAdjusting Glaze Expansion by Calculation to Solve ShiveringAlberta Slip, 20 Years of Substitution for Albany SlipAn Overview of Ceramic StainsAre You in Control of Your Production Process?Are Your Glazes Food Safe or are They Leachable?Attack on Glass: Corrosion Attack MechanismsBall Milling Glazes, Bodies, EngobesBinders for Ceramic BodiesBringing Out the Big Guns in Craze Control: MgO (G1215U)Can We Help You Fix a Specific Problem?Ceramic Glazes TodayCeramic Material NomenclatureCeramic Tile Clay Body FormulationChanging Our View of GlazesChemistry vs. Matrix Blending to Create Glazes from Native MaterialsConcentrate on One Good GlazeCopper Red GlazesCrazing and Bacteria: Is There a Hazard?Crazing in Stoneware Glazes: Treating the Causes, Not the SymptomsCreating a Non-Glaze Ceramic Slip or EngobeCreating Your Own Budget GlazeCrystal Glazes: Understanding the Process and MaterialsDeflocculants: A Detailed OverviewDemonstrating Glaze Fit Issues to StudentsDiagnosing a Casting Problem at a Sanitaryware PlantDrying Ceramics Without CracksDuplicating Albany SlipDuplicating AP Green FireclayElectric Hobby Kilns: What You Need to KnowFighting the Glaze DragonFiring Clay Test BarsFiring: What Happens to Ceramic Ware in a Firing KilnFirst You See It Then You Don't: Raku Glaze StabilityFixing a glaze that does not stay in suspensionFormulating a body using clays native to your areaFormulating a Clear Glaze Compatible with Chrome-Tin StainsFormulating a PorcelainFormulating Ash and Native-Material GlazesG1214M Cone 5-7 20x5 glossy transparent glazeG1214W Cone 6 transparent glazeG1214Z Cone 6 matte glazeG1916M Cone 06-04 transparent glazeGetting the Glaze Color You Want: Working With StainsGlaze and Body Pigments and Stains in the Ceramic Tile IndustryGlaze Chemistry Basics - Formula, Analysis, Mole%, UnityGlaze chemistry using a frit of approximate analysisGlaze Recipes: Formulate and Make Your Own InsteadGlaze Types, Formulation and Application in the Tile IndustryHaving Your Glaze Tested for Toxic Metal ReleaseHigh Gloss GlazesHire Us for a 3D Printing ProjectHow a Material Chemical Analysis is DoneHow desktop INSIGHT Deals With Unity, LOI and Formula WeightHow to Find and Test Your Own Native ClaysI have always done it this way!Inkjet Decoration of Ceramic TilesIs Your Fired Ware Safe?Leaching Cone 6 Glaze Case StudyLimit Formulas and Target FormulasLow Budget Testing of Ceramic GlazesMake Your Own Ball Mill StandMaking Glaze Testing ConesMonoporosa or Single Fired Wall TilesOrganic Matter in Clays: Detailed OverviewOutdoor Weather Resistant CeramicsPainting Glazes Rather Than Dipping or SprayingParticle Size Distribution of Ceramic PowdersPorcelain Tile, Vitrified TileRationalizing Conflicting Opinions About PlasticityRavenscrag Slip is BornRecylcing Scrap ClayReducing the Firing Temperature of a Glaze From Cone 10 to 6Setting up a Clay Testing Program in Your Company or StudioSimple Physical Testing of ClaysSingle Fire GlazingSoluble Salts in Minerals: Detailed OverviewSome Keys to Dealing With Firing CracksStoneware Casting Body RecipesSubstituting Cornwall StoneSuper-Refined Terra SigillataThe Chemistry, Physics and Manufacturing of Glaze FritsThe Effect of Glaze Fit on Fired Ware StrengthThe Four Levels on Which to View Ceramic GlazesThe Majolica Earthenware ProcessThe Potter's PrayerThe Right Chemistry for a Cone 6 Magnesia MatteThe Trials of Being the Only Technical Person in the ClubThe Whining Stops Here: A Realistic Look at Clay BodiesThose Unlabelled Bags and BucketsTiles and Mosaics for PottersToxicity of Firebricks Used in OvensTrafficking in Glaze RecipesUnderstanding Ceramic MaterialsUnderstanding Ceramic OxidesUnderstanding Glaze Slurry PropertiesUnderstanding the Deflocculation Process in Slip CastingUnderstanding the Terra Cotta Slip Casting Recipes In North AmericaUnderstanding Thermal Expansion in Ceramic GlazesUnwanted Crystallization in a Cone 6 GlazeUsing Dextrin, Glycerine and CMC Gum togetherVolcanic AshWhat Determines a Glaze's Firing Temperature?What is a Mole, Checking Out the MoleWhat is the Glaze Dragon?Where do I start in understanding glazes?Why Textbook Glazes Are So DifficultWorking with children A Textbook Cone 6 Matte Glaze With Problems
Description
Glazes must be completely melted to be functional, hard and strong. Many are not. This compares two glazes to make the difference clear.
Article
The picture below is a flow tester that was fired at cone 6. The tester itself is Plainsman M370. The glaze on the right is G1214W, a typical cone 6 transparent used by potters. It is fluxed by a boron sourcing frit. The glaze on the left is typical of what many use to achieve a matte. The recipe is:
| Nepheline Syenite | 40.00 |
| Dolomite | 15.00 |
| Whiting | 10.00 |
| Ball Clay | 20.00 |
| China Clay | 10.00 |
| Silica | 5.00 |
But this glaze is not flowing at all whereas the boron-fluxed glaze has run right to the bottom (and it is not even considered a highly fluid glaze). This simple comparison teaches us many things about glazes and even ourselves. Here are some of them.
- Cone 6 glazes require boron (from frits or gerstley borate) or zinc to melt (the one on the left has neither). Materials like feldspar, dolomite, whiting and talc just do not melt well at all at cone 6. If a glaze is not properly melted then it is not hard and strong and resistant to leaching and cutlery marking.
- Textbook glaze recipes often are junk. Unquestioned use of them demonstrates our willingness to accept something ridiculous just because it is in a book or on a web page. We need use common sense when looking at glaze recipes for cone 6 to determine if they are for real or impostors (the glaze on the left is actually really not a glaze, it is a porcelain). If there is no frit, no zinc, no gerstley borate, then a red this-likely-does-not-melt light is flashing.
- Glazes with high feldspar or nepheline syenite (40% is really high) are likely to craze. If this one does not craze it is simply because it has not melt enough for the sodium to impose its high thermal expansion on the glass.
- A cone 6 glaze with 30% clay (in this case ball clay and kaolin) and no boron is certainly not going to melt well because clay is refractory.
- True matte glazes have high alumina and low silica (which this has) but they also need to melt well to form a glass (which this does not). So this is just a matte because it is not melted.
- If a white-firing glaze has no zircon or tin oxide, then how can it be white? Something is wrong. In this case it is white simply because it is not melted.
- Since this does not melt, evaluating it on the basis of its chemistry would be invalid. Glaze chemistry theory depends on the glaze being melted to a homogeneous glass. Thus, in addition to knowing all about the chemistry, you need to have common sense on the recipe level also.
Understanding your glazes is so much better, especially when it comes to dealing with their problems (and this one would have plenty!).
Related Information
Before spending time trying online recipes, take a minute to do a sanity check on them

This picture has its own page with more detail, click here to see it.
This is a cone 6 GLFL test to compare melt-flow between a matte recipe, found online at a respected website, and a glaze we use often. Yes, it is matte. But why? Because it is not melted! Matte glazes used on functional surfaces need to melt well, they should flow like a glossy glaze. Even though this recipe has 40% nepheline syenite, lots of dolomite and calcium carbonate it is not melting. Yes, these are powerful fluxes, but at cone 10, not cone 6! To melt a cone 6 glaze boron, zinc or lithia are needed. Boron is the most common and best general-purpose melter for potters (it comes mainly in frits, Gerstley borate). The concept of a limit recipe applies here, the idea of eye-balling a recipe and quickly assessing if it is ridiculous or not.
A functional matte cone 6 glaze should melt as well as a glossy

This picture has its own page with more detail, click here to see it.
True functional mattes have fluid melts, like glossy glazes. They need this in order to develop a hard, non-scratching, durable glass. The mechanism of the G1214Z1 matte on the right is high Al2O3, it is actually melting more than the glossy G1214W on the left (this was fired between cone 5 and 6, it normally runs right off the runway).
Links