A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025A Low Cost Tester of Glaze Melt FluidityA One-speed Lab or Studio Slurry MixerA Textbook Cone 6 Matte Glaze With ProblemsAdjusting Glaze Expansion by Calculation to Solve ShiveringAlberta Slip, 20 Years of Substitution for Albany SlipAn Overview of Ceramic StainsAre You in Control of Your Production Process?Are Your Glazes Food Safe or are They Leachable?Attack on Glass: Corrosion Attack MechanismsBall Milling Glazes, Bodies, EngobesBinders for Ceramic BodiesBringing Out the Big Guns in Craze Control: MgO (G1215U)Can We Help You Fix a Specific Problem?Ceramic Glazes TodayCeramic Material NomenclatureCeramic Tile Clay Body FormulationChanging Our View of GlazesChemistry vs. Matrix Blending to Create Glazes from Native MaterialsConcentrate on One Good GlazeCopper Red GlazesCrazing and Bacteria: Is There a Hazard?Crazing in Stoneware Glazes: Treating the Causes, Not the SymptomsCreating a Non-Glaze Ceramic Slip or EngobeCreating Your Own Budget GlazeCrystal Glazes: Understanding the Process and MaterialsDeflocculants: A Detailed OverviewDemonstrating Glaze Fit Issues to StudentsDiagnosing a Casting Problem at a Sanitaryware PlantDrying Ceramics Without CracksDuplicating Albany SlipDuplicating AP Green FireclayElectric Hobby Kilns: What You Need to KnowFighting the Glaze DragonFiring Clay Test BarsFiring: What Happens to Ceramic Ware in a Firing KilnFirst You See It Then You Don't: Raku Glaze StabilityFixing a glaze that does not stay in suspensionFormulating a body using clays native to your areaFormulating a Clear Glaze Compatible with Chrome-Tin StainsFormulating a PorcelainFormulating Ash and Native-Material GlazesG1214M Cone 5-7 20x5 glossy transparent glazeG1214W Cone 6 transparent glazeG1214Z Cone 6 matte glazeG1916M Cone 06-04 transparent glazeGetting the Glaze Color You Want: Working With StainsGlaze and Body Pigments and Stains in the Ceramic Tile IndustryGlaze Chemistry Basics - Formula, Analysis, Mole%, UnityGlaze chemistry using a frit of approximate analysisGlaze Recipes: Formulate and Make Your Own InsteadGlaze Types, Formulation and Application in the Tile IndustryHaving Your Glaze Tested for Toxic Metal ReleaseHigh Gloss GlazesHire Us for a 3D Printing ProjectHow a Material Chemical Analysis is DoneHow desktop INSIGHT Deals With Unity, LOI and Formula WeightHow to Find and Test Your Own Native ClaysI have always done it this way!Inkjet Decoration of Ceramic TilesIs Your Fired Ware Safe?Leaching Cone 6 Glaze Case StudyLimit Formulas and Target FormulasLow Budget Testing of Ceramic GlazesMake Your Own Ball Mill StandMaking Glaze Testing ConesMonoporosa or Single Fired Wall TilesOrganic Matter in Clays: Detailed OverviewOutdoor Weather Resistant CeramicsPainting Glazes Rather Than Dipping or SprayingParticle Size Distribution of Ceramic PowdersPorcelain Tile, Vitrified TileRationalizing Conflicting Opinions About PlasticityRavenscrag Slip is BornRecylcing Scrap ClayReducing the Firing Temperature of a Glaze From Cone 10 to 6Setting up a Clay Testing Program in Your Company or StudioSimple Physical Testing of ClaysSingle Fire GlazingSoluble Salts in Minerals: Detailed OverviewSome Keys to Dealing With Firing CracksStoneware Casting Body RecipesSubstituting Cornwall StoneSuper-Refined Terra SigillataThe Chemistry, Physics and Manufacturing of Glaze FritsThe Effect of Glaze Fit on Fired Ware StrengthThe Four Levels on Which to View Ceramic GlazesThe Majolica Earthenware ProcessThe Potter's PrayerThe Right Chemistry for a Cone 6 Magnesia MatteThe Trials of Being the Only Technical Person in the ClubThe Whining Stops Here: A Realistic Look at Clay BodiesThose Unlabelled Bags and BucketsTiles and Mosaics for PottersToxicity of Firebricks Used in OvensTrafficking in Glaze RecipesUnderstanding Ceramic MaterialsUnderstanding Ceramic OxidesUnderstanding Glaze Slurry PropertiesUnderstanding the Deflocculation Process in Slip CastingUnderstanding the Terra Cotta Slip Casting Recipes In North AmericaUnderstanding Thermal Expansion in Ceramic GlazesUnwanted Crystallization in a Cone 6 GlazeUsing Dextrin, Glycerine and CMC Gum togetherVolcanic AshWhat Determines a Glaze's Firing Temperature?What is a Mole, Checking Out the MoleWhat is the Glaze Dragon?Where do I start in understanding glazes?Why Textbook Glazes Are So DifficultWorking with children
Diagnosing a Casting Problem at a Sanitaryware Plant
Description
A company using a rubbery casting slip and depending on outside technical support discovers how simple it is to fix a slip that is drastically wrong using simple testing.
Article
I joined a company that manufactured sanitaryware. It had been built and run by an overseas company who then sold it to a South African holding company. The plant was a conventional one, the slip being prepared in a sliphouse, the clays turned into slops using blungers, and a body slip made up and then filter pressed. The filtercakes were then reconstituted into a casting slip. This was the best way, rather than direct slip making, as the clays were crude and needed to be cleaned up first.
White glaze was produced at the plant, coloured glazes were bought in. Casting was by hand using casting benches and firing was carried out in electric tophat kilns.
When I arrived the slip was like porridge and casting times were long. It was something to watch casters handling separate cast rims, they flexed like rubber in their hands! I immediately had an idea what was wrong but needed to prove it. The original owners had used their overseas technical facilities and so the plant did not have a Lab to speak of. One test was being done - particle size by hydrometer, and that was wrong. So to investigate the slip problem I bought a torsion viscometer, a burette and stand, a small lab stirrer and a stopclock. Then I proceeded to do deflocculation curves on each clay. Of the four clays it became obvious that there were problems with two of them. One of them was a china clay obtained from a small company in the area. While it should have deflocculated easily, instead it gelled to the extent that I could invert the container of clay slip (with added deflocculant) and it stayed in place, not even shaking could remove it! The other clay was supplied by a brickworks and it also thickened rather than thinned as deflocculant was added, but not to the extent of the China clay. By now I definitely knew the problem was that of Montmorillonite in the clays, which causes gelling. I sent the clays for XRD analysis, reminding the laboratory to add glycerol to the them to cause the Monmorillonite to swell on its C-axis (otherwise it might not be detected). It was detected in both of the 2 clays.
The offending clays were replaced and the slip became fluid and the casting rate was much faster and the cast items were hard. A shorter body resulted but the casters soon adapted and the formulation continued to be used for years.
Monmorillonite contains Magnesium in the Brucite layer, I wondered how both of the errant clays, which were essentially kaolinitic, came to have Montmorillonite in them. I am not a Geologist but I reckoned that perhaps there was Magnesium containing rocks near to these clays. This turned out to be true, in the Cape there were such rocks exposed above the China clay deposit and only the clay near to the surface contained Montmorillonite. In addition, the brick clay was in a Dolomitic area.
 PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
|
By Peter Clowes
Got a Question?
Buy me a coffee and we can talk 
https://backup.digitalfire.com, All Rights Reserved
Privacy Policy