A ChatBot gives jaw-dropping glaze recipe advice - Jan 2025A Low Cost Tester of Glaze Melt FluidityA One-speed Lab or Studio Slurry MixerA Textbook Cone 6 Matte Glaze With ProblemsAdjusting Glaze Expansion by Calculation to Solve ShiveringAlberta Slip, 20 Years of Substitution for Albany SlipAn Overview of Ceramic StainsAre You in Control of Your Production Process?Are Your Glazes Food Safe or are They Leachable?Attack on Glass: Corrosion Attack MechanismsBall Milling Glazes, Bodies, EngobesBinders for Ceramic BodiesBringing Out the Big Guns in Craze Control: MgO (G1215U)Can We Help You Fix a Specific Problem?Ceramic Glazes TodayCeramic Material NomenclatureCeramic Tile Clay Body FormulationChanging Our View of GlazesChemistry vs. Matrix Blending to Create Glazes from Native MaterialsConcentrate on One Good GlazeCopper Red GlazesCrazing and Bacteria: Is There a Hazard?Crazing in Stoneware Glazes: Treating the Causes, Not the SymptomsCreating a Non-Glaze Ceramic Slip or EngobeCreating Your Own Budget GlazeCrystal Glazes: Understanding the Process and MaterialsDeflocculants: A Detailed OverviewDemonstrating Glaze Fit Issues to StudentsDiagnosing a Casting Problem at a Sanitaryware PlantDrying Ceramics Without CracksDuplicating Albany SlipDuplicating AP Green FireclayElectric Hobby Kilns: What You Need to KnowFighting the Glaze DragonFiring Clay Test BarsFiring: What Happens to Ceramic Ware in a Firing KilnFirst You See It Then You Don't: Raku Glaze StabilityFixing a glaze that does not stay in suspensionFormulating a body using clays native to your areaFormulating a Clear Glaze Compatible with Chrome-Tin StainsFormulating a PorcelainFormulating Ash and Native-Material GlazesG1214M Cone 5-7 20x5 glossy transparent glazeG1214W Cone 6 transparent glazeG1214Z Cone 6 matte glazeG1916M Cone 06-04 transparent glazeGetting the Glaze Color You Want: Working With StainsGlaze and Body Pigments and Stains in the Ceramic Tile IndustryGlaze Chemistry Basics - Formula, Analysis, Mole%, UnityGlaze chemistry using a frit of approximate analysisGlaze Recipes: Formulate and Make Your Own InsteadGlaze Types, Formulation and Application in the Tile IndustryHaving Your Glaze Tested for Toxic Metal ReleaseHigh Gloss GlazesHire Us for a 3D Printing ProjectHow a Material Chemical Analysis is DoneHow desktop INSIGHT Deals With Unity, LOI and Formula WeightHow to Find and Test Your Own Native ClaysI have always done it this way!Inkjet Decoration of Ceramic TilesIs Your Fired Ware Safe?Leaching Cone 6 Glaze Case StudyLimit Formulas and Target FormulasLow Budget Testing of Ceramic GlazesMake Your Own Ball Mill StandMaking Glaze Testing ConesMonoporosa or Single Fired Wall TilesOrganic Matter in Clays: Detailed OverviewOutdoor Weather Resistant CeramicsPainting Glazes Rather Than Dipping or SprayingParticle Size Distribution of Ceramic PowdersPorcelain Tile, Vitrified TileRationalizing Conflicting Opinions About PlasticityRavenscrag Slip is BornRecylcing Scrap ClayReducing the Firing Temperature of a Glaze From Cone 10 to 6Setting up a Clay Testing Program in Your Company or StudioSimple Physical Testing of ClaysSingle Fire GlazingSoluble Salts in Minerals: Detailed OverviewSome Keys to Dealing With Firing CracksStoneware Casting Body RecipesSubstituting Cornwall StoneSuper-Refined Terra SigillataThe Chemistry, Physics and Manufacturing of Glaze FritsThe Effect of Glaze Fit on Fired Ware StrengthThe Four Levels on Which to View Ceramic GlazesThe Majolica Earthenware ProcessThe Potter's PrayerThe Right Chemistry for a Cone 6 Magnesia MatteThe Trials of Being the Only Technical Person in the ClubThe Whining Stops Here: A Realistic Look at Clay BodiesThose Unlabelled Bags and BucketsTiles and Mosaics for PottersToxicity of Firebricks Used in OvensTrafficking in Glaze RecipesUnderstanding Ceramic MaterialsUnderstanding Ceramic OxidesUnderstanding Glaze Slurry PropertiesUnderstanding the Deflocculation Process in Slip CastingUnderstanding the Terra Cotta Slip Casting Recipes In North AmericaUnderstanding Thermal Expansion in Ceramic GlazesUnwanted Crystallization in a Cone 6 GlazeUsing Dextrin, Glycerine and CMC Gum togetherVolcanic AshWhat Determines a Glaze's Firing Temperature?What is a Mole, Checking Out the MoleWhat is the Glaze Dragon?Where do I start in understanding glazes?Why Textbook Glazes Are So DifficultWorking with children
Fixing a glaze that does not stay in suspension
Description
Fixing a glaze that does not suspend
Article
This was simple in INSIGHT.
First, it has no clay, there is no way it is going to stay in suspension. EPK is a great clay for glazes, it supplies alumina and silica. I put this glaze into INSIGHT and then duplicated it so I had two identical recipes side-by-side.
Then I killed the feldspar (it supplies silica, alumina and sodium). I then added Frit 3110 which is similar to feldspar but has almost no alumina. I tuned its amount to match the Na2O up, then I added EPK and increased it until the Al2O3 matched. Then I increased the Silica to match the SiO2 up.
This is the same process as is described in the lessons section of the INSIGHT manual. I got this. Fined tuning is still needed but you get the idea. You might try using ball clay instead of kaolin, minimum kaolin is usually about 15%. I was able to get 15% ball clay by dropping the bentonite and also using Frit 3110 to supply the K2O and Na2O instead of the feldspar. The key is that the changed recipe has the same chemistry but uses a different mix of ingredients to supply it. Try this recipe and let me know what happens.
Adjust the rutile to be the same percentage as the original and use the copper at the same percentage as well. I don't think this adds up to 100, so keep that in mind.
4.44 Whiting
5.56 Talc
29.89 Ferro Frit 3134
34.89 Silica #325
1.11 Bentonite
6.67 Rutile
17.00 Frit 3110
11.00 EP Kaolin
-------8<-- ------
Hi Tony, thanks for getting back to me, thisa is the recipe from Bill van Gilder that is settling out. I mixed a 10,000 gram batch:
Custer fekdspar 2200
Whiting 400
Talc 500
Ferro Frit 3134 2600
Silica #325 2600
Bentonite 100
Rutile 600
Copper carb 400
I mixed and seived with 80 mesh screen. After several dips it started acting strange, like it wasn't covering very heavily. It would be transparent sometimes and then in spots would be heavy enough to give abeautiful glaze. So I added about 1 1/2 teaspoons Gum solution. That helped some but I still must mix alot before using. I emailed Bill VG about this but never got an answer so I really appreciate You answering me. Restores my faith in man. I just might have to get this program of yours even if I dont understand it. If you have time I will send you the Pete Pinnell recipe also, he also didnt answer my questions, you might turn about to be the new glaze God.
Peggy Mahoney
 PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
|
By Tony Hansen Follow me on
 |  |
Got a Question?
Buy me a coffee and we can talk 
https://backup.digitalfire.com, All Rights Reserved
Privacy Policy