3547 | 3487 | 254 | 3845 | 3703 | 203 | 932 | 2742 | 2743 | 809 | 1743 | 1744 | 285 | 290 | 1598 | 1340 | 380 | 765 | 2558 | 2559 | 1393 | 1927 | 1928 | 1642 | 2892 | 2026 | 2620 | 2027 | 566 | 1139 | 1692 | 2626 | 1181 | 1182 | 2872 | 1549 | 1415 | 388 | 1620 | 2604 | 701 | 3055 | 1127 | 958 | 2992 | 2993 | 808 | 2874 | 2873 | 1847 | 1575 | 586 | 207 | 673 | 1293 | 1071 | 1602 | 1095 | 2855 | 2853 | 2854 | 637 | 2409 | 2410 | 720 | 3051 | 1399 | 1440 | 1383 | 695 | 2768 | 2767 | 2074 | 2686 | 492 | 480 | 495 | 310 | 313 | 473 | 474 | 450 | 314 | 475 | 521 | 455 | 486 | 469 | 481 | 425 | 1129 | 466 | 467 | 482 | 316 | 1132 | 468 | 445 | 446 | 477 | 448 | 472 | 315 | 471 | 439 | 311 | 484 | 447 | 1325 | 440 | 518 | 442 | 378 | 443 | 1288 | 444 | 1283 | 1374 | 1171 | 461 | 420 | 465 | 424 | 451 | 464 | 462 | 487 | 1270 | 423 | 1177 | 485 | 1275 | 459 | 317 | 449 | 419 | 370 | 1441 | 458 | 318 | 319 | 418 | 1410 | 1372 | 320 | 322 | 497 | 371 | 308 | 309 | 1184 | 383 | 323 | 1161 | 324 | 456 | 417 | 1439 | 1286 | 1371 | 496 | 531 | 1191 | 501 | 379 | 498 | 409 | 305 | 325 | 1151 | 357 | 493 | 1136 | 361 | 437 | 299 | 500 | 326 | 1336 | 457 | 327 | 491 | 1377 | 441 | 520 | 503 | 1150 | 298 | 1396 | 399 | 1446 | 328 | 411 | 1135 | 470 | 505 | 1178 | 1376 | 306 | 504 | 408 | 1149 | 1153 | 483 | 304 | 507 | 488 | 329 | 1173 | 489 | 1266 | 330 | 302 | 506 | 1186 | 333 | 331 | 372 | 1362 | 303 | 1426 | 1375 | 1373 | 344 | 400 | 404 | 334 | 1188 | 332 | 301 | 369 | 463 | 413 | 312 | 490 | 1413 | 512 | 453 | 335 | 511 | 510 | 509 | 502 | 406 | 416 | 407 | 494 | 365 | 1154 | 508 | 300 | 1433 | 541 | 1313 | 363 | 428 | 381 | 452 | 1145 | 476 | 336 | 460 | 426 | 1287 | 540 | 427 | 1390 | 1284 | 429 | 1280 | 430 | 307 | 431 | 337 | 433 | 454 | 516 | 1155 | 1156 | 339 | 1157 | 544 | 434 | 1141 | 1384 | 1137 | 543 | 542 | 435 | 1389 | 546 | 1273 | 1416 | 438 | 1276 | 382 | 1332 | 1326 | 1977 | 1978 | 1774 | 2569 | 2570 | 1508 | 1007 | 1785 | 1786 | 598 | 3033 | 793 | 1464 | 2300 | 2301 | 1660 | 1133 | 786 | 206 | 204 | 1189 | 2577 | 2578 | 2579 | 1537 | 1534 | 1536 | 282 | 3170 | 986 | 2339 | 700 | 2987 | 2988 | 2955 | 436 | 1833 | 2341 | 2342 | 795 | 2470 | 2471 | 1843 | 2885 | 2886 | 2887 | 340 | 260 | 1180 | 3305 | 368 | 1698 | 73 | 105 | 27 | 168 | 106 | 159 | 199 | 28 | 156 | 232 | 102 | 107 | 163 | 1467 | 1590 | 847 | 2412 | 1290 | 1605 | 1826 | 2960 | 1479 | 1573 | 1615 | 1019 | 2978 | 922 | 2979 | 23 | 25 | 1460 | 1334 | 390 | 2453 | 2454 | 1689 | 249 | 1948 | 291 | 1364 | 205 | 1969 | 2469 | 2958 | 766 | 2959 | 919 | 2003 | 3034 | 3035 | 3036 | 1322 | 1980 | 1981 | 1982 | 1571 | 2820 | 37 | 2437 | 1341 | 1418 | 2543 | 1732 | 2641 | 2088 | 2087 | 1121 | 2256 | 2842 | 2843 | 2844 | 2098 | 2099 | 2100 | 2102 | 1296 | 2130 | 2131 | 375 | 169 | 479 | 36 | 410 | 157 | 161 | 103 | 1176 | 201 | 2966 | 1466 | 591 | 892 | 2601 | 1172 | 1010 | 2822 | 2823 | 966 | 1450 | 755 | 3134 | 3136 | 3135 | 112 | 113 | 135 | 138 | 139 | 140 | 141 | 623 | 1750 | 2621 | 1457 | 212 | 1728 | 1908 | 1909 | 412 | 283 | 1552 | 791 | 2952 | 2953 | 639 | 1388 | 2651 | 668 | 1430 | 2605 | 1431 | 1432 | 1434 | 901 | 2020 | 2021 | 1307 | 1308 | 1477 | 1300 | 1310 | 1301 | 1309 | 1378 | 1379 | 1304 | 1303 | 1312 | 1311 | 1305 | 1302 | 1148 | 856 | 2539 | 115 | 1424 | 193 | 194 | 2022 | 677 | 240 | 111 | 236 | 780 | 1111 | 831 | 2012 | 2896 | 698 | 744 | 2890 | 1008 | 2891 | 2791 | 2792 | 2793 | 672 | 2109 | 235 | 1369 | 2045 | 2044 | 1417 | 631 | 132 | 134 | 145 | 147 | 150 | 1142 | 2980 | 792 | 2981 | 1738 | 1757 | 1758 | 1739 | 1759 | 1760 | 2061 | 1849 | 2357 | 1032 | 2871 | 1733 | 1472 | 1123 | 2191 | 2192 | 1187 | 1470 | 1096 | 657 | 2707 | 1442 | 1411 | 1289 | 270 | 269 | 1412 | 712 | 725 | 770 | 1492 | 2757 | 2758 | 751 | 2856 | 2857 | 2510 | 2715 | 2716 | 945 | 1092 | 2181 | 2182 | 548 | 3093 | 3094 | 833 | 2183 | 2184 | 800 | 1766 | 1767 | 523 | 2760 | 1281 | 665 | 1527 | 499 | 1595 | 1012 | 3166 | 3167 | 2635 | 2636 | 3000 | 1737 | 1556 | 1323 | 1324 | 1497 | 1493 | 2189 | 2190 | 1482 | 1495 | 1112 | 2304 | 2303 | 1496 | 2193 | 2194 | 3111 | 898 | 3112 | 213 | 653 | 1299 | 1349 | 2201 | 2202 | 651 | 2173 | 3077 | 3078 | 3079 | 2923 | 2924 | 1099 | 1292 | 1343 | 1499 | 1769 | 2212 | 2213 | 909 | 693 | 669 | 366 | 2221 | 2607 | 1179 | 711 | 391 | 2881 | 547 | 2882 | 142 | 143 | 151 | 152 | 153 | 154 | 155 | 2917 | 2916 | 2918 | 2230 | 2231 | 1023 | 2232 | 2233 | 1507 | 1152 | 759 | 2234 | 1274 | 1498 | 1500 | 343 | 667 | 2838 | 2839 | 1501 | 200 | 622 | 2631 | 2632 | 1093 | 130 | 131 | 2638 | 144 | 2568 | 128 | 129 | 2241 | 634 | 2242 | 1110 | 1485 | 1503 | 663 | 1484 | 3355 | 279 | 670 | 1579 | 2259 | 1504 | 8 | 9 | 1385 | 2037 | 2038 | 364 | 578 | 3397 | 276 | 367 | 271 | 274 | 272 | 1350 | 902 | 2274 | 1113 | 845 | 2717 | 550 | 346 | 1788 | 1790 | 2279 | 2280 | 655 | 1789 | 1403 | 278 | 1386 | 3127 | 775 | 3128 | 703 | 2285 | 1425 | 202 | 692 | 2291 | 2292 | 781 | 934 | 2204 | 3091 | 3090 | 3092 | 78 | 114 | 1195 | 1196 | 1197 | 1198 | 1199 | 1200 | 1201 | 1203 | 1204 | 1205 | 1206 | 1207 | 1208 | 1209 | 1210 | 1211 | 1212 | 1193 | 1213 | 1214 | 1215 | 1216 | 1217 | 1218 | 1219 | 1220 | 1221 | 1222 | 1223 | 1192 | 1224 | 1225 | 1226 | 1228 | 1229 | 1230 | 1231 | 1232 | 1233 | 1234 | 1235 | 1236 | 1239 | 1238 | 1240 | 1237 | 1241 | 1242 | 1243 | 1244 | 1202 | 1227 | 1245 | 1194 | 1246 | 1247 | 1248 | 1249 | 1250 | 1251 | 1252 | 1253 | 1254 | 1255 | 1256 | 1257 | 1258 | 1259 | 1449 | 2852 | 2851 | 691 | 778 | 1067 | 2105 | 2990 | 2989 | 2991 | 579 | 3061 | 3060 | 736 | 3067 | 3066 | 2903 | 2904 | 2905 | 1033 | 2831 | 2832 | 1657 | 614 | 995 | 678 | 2985 | 1119 | 2986 | 2827 | 2828 | 2826 | 1435 | 2188 | 1328 | 392 | 394 | 395 | 403 | 387 | 1131 | 386 | 385 | 384 | 118 | 119 | 398 | 401 | 1130 | 402 | 396 | 1128 | 1330 | 555 | 557 | 1183 | 1392 | 1278 | 1816 | 2320 | 2321 | 1819 | 2327 | 1818 | 2324 | 2325 | 1331 | 2328 | 2789 | 195 | 1306 | 1558 | 784 | 3118 | 1057 | 3119 | 723 | 823 | 2332 | 761 | 1823 | 1824 | 737 | 1812 | 937 | 1073 | 2333 | 2334 | 104 | 238 | 1643 | 948 | 3076 | 1933 | 1934 | 1935 | 34 | 1829 | 2515 | 1190 | 763 | 570 | 3472 | 3074 | 3075 | 217 | 1506 | 997 | 2345 | 2346 | 1677 | 2347 | 1088 | 1447 | 624 | 676 | 2806 | 674 | 2780 | 659 | 724 | 688 | 61 | 209 | 210 | 211 | 1656 | 687 | 2293 | 1848 | 1402 | 1401 | 3080 | 702 | 1865 | 1866 | 1867 | 662 | 730 | 569 | 220 | 1089 | 1868 | 2650 | 2608 | 694 | 756 | 2804 | 1143 | 605 | 2652 | 642 | 3064 | 3065 | 707 | 757 | 1872 | 1720 | 1721 | 1873 | 241 | 545 | 1419 | 746 | 1509 | 748 | 713 | 1370 | 1771 | 602 | 764 | 170 | 478 | 160 | 1185 | 158 | 1090 | 595 | 1468 | 1400 | 527 | 528 | 529 | 530 | 532 | 533 | 534 | 535 | 536 | 538 | 537 | 539 | 1062 | 2390 | 2391 | 868 | 2994 | 2995 | 1321 | 1320 | 1160 | 824 | 2370 | 2406 | 1335 | 98 | 99 | 706 | 903 | 2883 | 2884 | 1272 | 101 | 3011 | 3012 | 3013 | 1260 | 1887 | 1888 | 1262 | 2419 | 2511 | 647 | 618 | 728 | 1100 | 192 | 397 | 680 | 2787 | 2786 | 2788 | 553 | 341 | 1444 | 1443 | 1505 | 1164 | 1165 | 1166 | 1167 | 1168 | 1169 | 782 | 876 | 225 | 635 | 3168 | 3169 | 1147 | 345 | 31 | 33 | 1428 | 1557 | 32 | 259 | 1103 | 558 | 783 | 277 | 2439 | 2440 | 1900 | 1102 | 1608 | 1525 | 2448 | 2449 | 1405 | 1068 | 2501 | 697 | 613 | 645 | 2065 | 2066 | 3673 | 749 | 1365 | 1366 | 20 | 18 | 17 | 19 | 1576 | 2460 | 718 | 2461 | 2462 | 2609 | 393 | 704 | 721 | 2465 | 742 | 1124 | 1945 | 2622 | 587 | 2658 | 1764 | 1763 | 1741 | 607 | 1017 | 1953 | 1954 | 1140 | 726 | 1318 | 719 | 3373 | 733 | 2630 | 754 | 2525 | 2526 | 1053 | 2805 | 2090 | 3383 | 2835 | 2836 | 2837 | 709 | 2167 | 2168 | 658 | 656 | 1568 | 1474 | 1327 | 1158 | 972 | 1966 | 2814 | 2813 | 2815 | 2698 | 2697 | 2699 | 1971 | 1972 | 1973 | 2472 | 2865 | 2866 | 2867 | 2846 | 2845 | 2847 | 295 | 297 | 1777 | 3156 | 3157 | 1984 | 1983 | 1985 | 1987 | 1986 | 1988 | 3037 | 975 | 3038 | 758 | 2807 | 2808 | 788 | 2533 | 2534 | 358 | 359 | 360 | 3045 | 3046 | 3047 | 785 | 2614 | 2615 | 1382 | 3017 | 3016 | 164 | 1550 | 1600 | 517 | 519 | 522 | 524 | 526 | 1098 | 1039 | 2005 | 2006 | 7 | 2967 | 741 | 1261 | 3733 | 2479 | 2478 | 2000 | 3116 | 912 | 2484 | 1337 | 722 | 2863 | 2862 | 2864 | 953 | 1892 | 1893 | 1531 | 162 | 1294 | 2490 | 1006 | 10 | 11 | 559 | 3048 | 1530 | 1138 | 1478 | 923 | 3009 | 3010 | 773 | 1703 | 2492 | 2493 | 2458 | 752 | 629 | 422 | 2094 | 2093 | 2095 | 1452 | 2496 | 2497 | 1553 | 1106 | 1489 | 772 | 3005 | 3004 | 3006 | 281 | 1097 | 2111 | 2112 | 2113 | 1358 | 1118 | 1404 | 1398 | 2996 | 2997 | 2998 | 1513 | 2122 | 2121 | 1514 | 1515 | 2129 | 2128 | 1144 | 1661 | 753 | 432 | 1361 | 682 | 2507 | 2508 | 373 | 374 | 377 | 376 | 239 | 1516 | 2143 | 2142 | 2144 | 679 | 787 | 2868 | 2869 | 1753 | 3043 | 3044 | 2849 | 2848 | 2850 | 621 | 3103 | 3102 | 3104 | 1974 | 1975 | 1976 | 2858 | 2860 | 2859 | 965 | 3143 | 3144 | 2824 | 858 | 2999 | 180 | 175 | 181 | 182 | 183 | 174 | 178 | 38 | 165 | 1271 | 769 | 803 | 1529 | 1134 | 2153 | 2154 | 643 | 3109 | 3110 | 2155 | 2156 | 2157 | 1101 | 2158 | 2825 | 3201 | 1613 | 3483 | 841 | 2521 | 2522 | 888 | 2523 | 2524 | 1597 | 284 | 1599 | 955 | 1745 | 3202 | 974 | 2600 | 2599 | 743 | 2694 | 2708 | 3702 | 1616 | 3500 | 2688 | 3557 | 632 | 1748 | 1913 | 3749 | 1749 | 1917 | 1916 | 1778 | 2257 | 2798 | 2797 | 805 | 1589 | 3801 | 3504 | 3642 | 681 | 2563 | 2203 | 3672 | 3644 | 2551 | 2552 | 1342 | 2591 | 675 | 2687 | 2030 | 2149 | 2150 | 849 | 2947 | 2948 | 1670 | 907 | 2042 | 2043 | 3602 | 1069 | 2051 | 2949 | 2951 | 2950 | 3724 | 3725 | 3726 | 3727 | 3721 | 3303 | 3755 | 3549 | 3454 | 684 | 2265 | 3792 | 3793 | 3455 | 3714 | 3735 | 839 | 1762 | 1263 | 1277 | 626 | 2659 | 2660 | 3754 | 3129 | 879 | 3130 | 3179 | 3768 | 1523 | 1663 | 1688 | 3681 | 3380 | 3206 | 3506 | 3507 | 3596 | 3330 | 3376 | 1456 | 1970 | 2790 | 3279 | 3278 | 3280 | 3281 | 3282 | 878 | 3809 | 1631 | 2819 | 3403 | 1583 | 3740 | 2684 | 3456 | 2706 | 774 | 3510 | 565 | 2185 | 2186 | 1448 | 3319 | 1751 | 2187 | 2582 | 3605 | 3367 | 3341 | 3647 | 641 | 3272 | 3683 | 1780 | 1682 | 3356 | 696 | 1957 | 2243 | 2244 | 3662 | 3567 | 3457 | 3880 | 963 | 2536 | 2946 | 2205 | 2206 | 906 | 2956 | 3302 | 971 | 2834 | 3421 | 3165 | 1655 | 2769 | 1421 | 3518 | 1644 | 3519 | 3476 | 1673 | 1653 | 3445 | 1582 | 1654 | 1475 | 3171 | 3691 | 3296 | 3295 | 3798 | 1647 | 1645 | 1650 | 1652 | 1648 | 1646 | 1651 | 1649 | 3194 | 3293 | 3292 | 3291 | 3796 | 3797 | 1268 | 342 | 1380 | 3400 | 3634 | 1414 | 167 | 3430 | 1679 | 3585 | 389 | 3435 | 3739 | 3616 | 3419 | 3588 | 1159 | 1269 | 1709 | 3434 | 1352 | 414 | 3189 | 689 | 2800 | 2801 | 1560 | 3404 | 601 | 1770 | 2216 | 2217 | 2218 | 1054 | 2450 | 1045 | 2909 | 2910 | 3753 | 628 | 2224 | 2225 | 3521 | 572 | 2925 | 2926 | 2499 | 2722 | 837 | 2237 | 3140 | 3141 | 3142 | 3505 | 3236 | 1565 | 3650 | 3508 | 3218 | 1108 | 1999 | 3712 | 1577 | 1458 | 1282 | 2672 | 1483 | 1381 | 1717 | 3477 | 3271 | 1669 | 3234 | 3266 | 3393 | 3192 | 1473 | 3414 | 3678 | 1547 | 3388 | 3493 | 3638 | 1491 | 3237 | 1574 | 3212 | 1684 | 3375 | 1584 | 1554 | 1528 | 1526 | 1566 | 1596 | 3358 | 3688 | 3211 | 1480 | 3190 | 1667 | 1541 | 3545 | 1666 | 2625 | 1639 | 1569 | 1535 | 3233 | 3394 | 3353 | 1691 | 3770 | 1329 | 2647 | 2238 | 2888 | 979 | 2889 | 2911 | 3760 | 1610 | 3571 | 921 | 3756 | 3197 | 1718 | 3366 | 3100 | 592 | 3101 | 3458 | 3632 | 3629 | 3572 | 3598 | 3527 | 589 | 2270 | 2271 | 993 | 2877 | 2878 | 2927 | 3306 | 3307 | 3777 | 3309 | 3308 | 3759 | 3599 | 3301 | 1471 | 3515 | 3548 | 3836 | 3512 | 3637 | 3633 | 2349 | 2350 | 1633 | 1126 | 2645 | 3649 | 3440 | 3876 | 3668 | 1729 | 2774 | 2773 | 927 | 2580 | 3087 | 3088 | 3089 | 3377 | 956 | 1799 | 1800 | 3820 | 3528 | 599 | 2682 | 2683 | 2576 | 3685 | 3624 | 3838 | 859 | 3007 | 3008 | 3198 | 603 | 2648 | 2649 | 3390 | 1122 | 2310 | 2311 | 1820 | 2329 | 2669 | 3731 | 3368 | 3407 | 3422 | 1436 | 1437 | 1544 | 3402 | | 3646 | 1593 | 3316 | 3313 | 3315 | 3406 | 3317 | 1524 | 1713 | 3426 | 3460 | 1454 | 1420 | 1581 | 1521 | 3423 | 3175 | 2565 | 2595 | 1588 | 1640 | 1455 | 3429 | 1459 | 1461 | 2710 | 3427 | 2779 | 2581 | 3418 | 1708 | 1548 | 1551 | 1463 | 1538 | 1572 | 3446 | 3300 | 2709 | 1562 | 3590 | 1060 | 1821 | 1822 | 861 | 2176 | 2547 | 2548 | 3565 | 3498 | 3707 | 3391 | 1707 | 3473 | 3056 | 3057 | 3459 | 3627 | 3604 | 3747 | 3610 | 2348 | 1845 | 3335 | 3214 | 2776 | 2778 | 2777 | 1701 | 3606 | 776 | 1863 | 1864 | 2723 | 2724 | 2725 | 853 | 2505 | 3561 | 1570 | 3480 | 1115 | 2368 | 2367 | 3290 | 1869 | 1870 | 3586 | 1871 | 2363 | 2364 | 2976 | 2977 | 1874 | 1875 | 762 | 2165 | 2166 | 2337 | 2338 | 3708 | 2123 | 2124 | 2713 | 2714 | 1714 | 2772 | 714 | 2740 | 2741 | 3667 | 1016 | 1632 | 2537 | 734 | 2538 | 560 | 2666 | 3191 | 2392 | 2393 | 1879 | 2394 | 2395 | 2906 | 2907 | 2908 | 1880 | 1881 | 3304 | 2398 | 2399 | 2400 | 3263 | 3563 | 3328 | 2247 | 1776 | 2248 | 777 | 3014 | 3015 | 2407 | 2408 | 1884 | 1885 | 797 | 2982 | 2983 | 1886 | 2416 | 2417 | 739 | 2418 | 2119 | 2703 | 2704 | 3593 | 1623 | 2424 | 3775 | 2893 | 2895 | 2894 | 1791 | 1585 | 3378 | 3475 | 611 | 2433 | 2432 | 2875 | 3494 | 1630 | 3556 | 2442 | 2443 | 2444 | 3329 | 2451 | 3287 | 3656 | 2670 | 2671 | 1700 | 1929 | 1930 | 857 | 2964 | 2436 | 3261 | 750 | 1932 | 1931 | 3339 | 2596 | 2696 | 790 | 2733 | 2734 | 1768 | 1665 | 883 | 1808 | 1809 | 3711 | 3441 | 3514 | 3560 | 1959 | 1960 | 2468 | 3072 | 826 | 3073 | 1486 | 3546 | 3531 | 581 | 2618 | 2619 | 844 | 2473 | 2474 | 3570 | 3786 | 3659 | 3669 | 1765 | 2685 | 3568 | 3529 | 3479 | 3113 | 3114 | 3115 | 1680 | 1423 | 3311 | 3713 | 3587 | 1086 | 2480 | 913 | 2783 | 3185 | 3641 | 3850 | 3849 | 3734 | 3758 | 575 | 2653 | 2654 | 3215 | 1851 | 1852 | 1853 | 992 | 1844 | 3332 | 3657 | 3615 | 3631 | 3736 | 593 | 2711 | 2712 | 3682 | 3365 | 939 | 2069 | 3172 | 2070 | 2071 | 1726 | 2556 | 2557 | 3343 | 2730 | 3542 | 1517 | 3709 | 1591 | 2085 | 2086 | 644 | 2089 | 3664 | 1629 | 3496 | 3520 | 3495 | 2500 | 940 | 2164 | 3352 | 2673 | 3651 | 2127 | 2504 | 3181 | 2506 | 1612 | 3174 | 1539 | 2145 | 2146 | 1716 | 3364 | 3677 | 648 | 2139 | 3544 | 3543 | 2147 | 2148 | 3275 | 1611 | 3569 | 3283 | 871 | 3063 | 3062 | 649 | 1742 | 3452 | 633 | 1925 | 1926 | 931 | 2612 | 1911 | 1910 | 3369 | 227 | 2598 | 2597 | 3069 | 3070 | 3071 | 3684 | 3347 | 3337 | 652 | 3049 | 3050 | 1921 | 1922 | 893 | 2527 | 811 | 2602 | 127 | 2531 | 2532 | 920 | 2744 | 2745 | 1746 | 615 | 1747 | 1170 | 2728 | 2729 | 789 | 2549 | 2550 | 3385 | 3226 | 3746 | 771 | 2262 | 2261 | 3676 | 3232 | 3482 | 1624 | 3409 | 3829 | 3433 | 3523 | 3320 | 3744 | 3525 | 3522 | 3432 | 3689 | 3625 | 3690 | 3574 | 3621 | 3524 | 3359 | 1609 | 1637 | 2818 | 1923 | 1924 | 1074 | 556 | 2962 | 2963 | 816 | 3123 | 3124 | 3209 | 3210 | 732 | 1914 | 1915 | 1022 | 2561 | 2560 | 806 | 3623 | 1719 | 1542 | 3613 | 1731 | 2661 | 2662 | 2784 | 2785 | 2693 | 3354 | 627 | 2901 | 2902 | 1991 | 2475 | 3517 | 1011 | 2542 | 1035 | 2135 | 2136 | 3449 | 3370 | 3345 | 630 | 2024 | 2025 | 1683 | 2028 | 779 | 2031 | 2032 | 2033 | 2034 | 2055 | 1338 | 1339 | 2463 | 2039 | 812 | 2535 | 1734 | 2041 | 3503 | 2049 | 2050 | 2973 | 2974 | 2975 | 3640 | 3674 | 810 | 3660 | 1690 | 908 | 1078 | 1810 | 3439 | 1811 | 3227 | 933 | 2056 | 2057 | 2058 | 2897 | 580 | 3230 | 561 | 2001 | 2002 | 745 | 2059 | 2060 | 1740 | 1761 | 2642 | 836 | 2326 | 3203 | 3526 | 2833 | 832 | 2062 | 2063 | 1061 | 2064 | 3497 | 1488 | 3448 | 924 | 2253 | 827 | 2163 | 3095 | 3097 | 3096 | 3148 | 3149 | 3147 | 1291 | 3607 | 3221 | 3199 | 3274 | 1564 | 802 | 1964 | 1686 | 1687 | 2170 | 2750 | 2751 | 1070 | 2174 | 2175 | 1429 | 1919 | 1920 | 2177 | 2178 | 3177 | 727 | 3276 | 951 | 3031 | 3032 | 1075 | 2434 | 2435 | 3655 | 2802 | 2803 | 2663 | 2664 | 571 | 2606 | 77 | 3611 | 1754 | 2518 | 2519 | 2520 | 3705 | 870 | 3025 | 1494 | 640 | 2195 | 3489 | 2764 | 3228 | 911 | 2199 | 2765 | 2200 | 2766 | 798 | 573 | 2761 | 2762 | 747 | 2378 | 2379 | 1736 | 2048 | 872 | 2564 | 2207 | 2208 | 961 | 2209 | 2210 | 2211 | 710 | 2689 | 2690 | 1675 | 896 | 2196 | 3053 | 2695 | 1532 | 3468 | 3351 | 1116 | 2782 | 3219 | 1699 | 1702 | 2219 | 2220 | 2222 | 2223 | 735 | 2180 | 1705 | 2226 | 1704 | 2227 | 3200 | 3743 | 1603 | 2228 | 2229 | 1021 | 2840 | 2841 | 3256 | 3250 | 3251 | 3253 | 3254 | 3255 | 3257 | 3252 | 2401 | 2236 | 1319 | 1772 | 1773 | 3841 | 3264 | 3501 | 1387 | 2633 | 2634 | 2239 | 1481 | 2566 | 2567 | 952 | 2344 | 2240 | 1662 | 760 | 2245 | 2246 | 3204 | 3384 | 3636 | 3732 | 3862 | 3864 | 3866 | 3877 | 3863 | 3821 | 3861 | 3865 | 3860 | 3859 | 3839 | 3854 | 3852 | 3840 | 3853 | 3774 | 1775 | 2571 | 2249 | 2250 | 3294 | 2251 | 2252 | 1175 | 3699 | 699 | 2254 | 799 | 3098 | 3099 | 2627 | 1059 | 2258 | 981 | 2260 | 3371 | 2264 | 2263 | 3562 | 3488 | 1782 | 1784 | 1783 | 3348 | 3622 | 2679 | 2680 | 2681 | 2572 | 2573 | 3761 | 3386 | 3387 | 794 | 2273 | 2574 | 2281 | 2282 | 1792 | 2277 | 2278 | 3235 | 1049 | 2275 | 2283 | 2284 | 3628 | 1671 | 3752 | 2286 | 2288 | 3131 | 3133 | 3132 | 3382 | 1793 | 2289 | 2290 | 1586 | 1080 | 1795 | 2491 | 3577 | 3579 | 3578 | 3580 | 2294 | 636 | 1796 | 1163 | 661 | 2266 | 2913 | 2267 | 2914 | 1297 | 880 | 2295 | 910 | 2590 | 2296 | 2297 | 2298 | 2299 | 768 | 596 | 1797 | 2718 | 2719 | 1798 | 3715 | 946 | 2702 | 2794 | 2795 | 1802 | 1803 | 1804 | 1046 | 2585 | 1055 | 600 | 588 | 2732 | 2575 | 3137 | 3138 | 3139 | 3745 | 2305 | 3028 | 3029 | 3030 | 2306 | 549 | 2035 | 2036 | 964 | 3039 | 3040 | 1020 | 3023 | 1091 | 2307 | 2308 | 1619 | 1353 | 1807 | 2309 | 405 | 3258 | 2312 | 2613 | 3081 | 1451 | 1814 | 2313 | 1839 | 2314 | 1838 | 1604 | 1832 | 2316 | 2318 | 2317 | 2319 | 1114 | 2315 | 35 | 3381 | 1627 | 3643 | 1490 | 2588 | 2589 | 2739 | 2928 | 1013 | 2323 | 984 | 2322 | 1058 | 3297 | 3350 | 3490 | 3491 | 3530 | 3374 | 3748 | 3357 | 3601 | 3827 | 3826 | 3833 | 3828 | 3831 | 3824 | 3825 | 3815 | 3842 | 3837 | 3835 | 3872 | 3834 | 3883 | 3846 | 3851 | 3855 | 3848 | 3881 | 3871 | 3873 | 3875 | 3856 | 3882 | 3858 | 3879 | 3868 | 3857 | 3750 | 3773 | 3794 | 3763 | 3767 | 3771 | 3762 | 3766 | 3765 | 3776 | 3769 | 3784 | 3780 | 3779 | 3782 | 3778 | 3788 | 3844 | 3787 | 3802 | 3803 | 3805 | 3832 | 3804 | 3808 | 3630 | 3843 | 3812 | 3813 | 3807 | 3814 | 3811 | 2330 | 2331 | 3178 | 1625 | 890 | 968 | 1828 | 2336 | 2335 | 3612 | 2810 | 2811 | 2812 | 2705 | 1622 | 2340 | 2646 | 941 | 2516 | 1830 | 2517 | 1831 | 1834 | 1835 | 1298 | 2937 | 2938 | 2376 | 1836 | 1837 | 1840 | 1841 | 1561 | 1546 | 2879 | 2880 | 1614 | 3310 | 3471 | 767 | 3161 | 3162 | 2084 | 2829 | 2830 | 1117 | 2302 | 3026 | 3027 | 3334 | 3340 | 814 | 3298 | 3299 | 1333 | 3665 | 1715 | 3645 | 3806 | 3224 | 2351 | 1264 | 2584 | 3614 | 1265 | 2354 | 2355 | 3453 | 2431 | 619 | 551 | 1285 | 2358 | 1850 | 2359 | 2360 | 3346 | 2361 | 3738 | 3717 | 3719 | 3781 | 3205 | 2529 | 2530 | 1855 | 1856 | 1857 | 3635 | 3704 | 1858 | 1860 | 1859 | 987 | 1861 | 1862 | 2971 | 2970 | 2972 | 3229 | 2781 | 2720 | 2721 | 3222 | 3652 | 1672 | 1787 | 3262 | 1051 | 2362 | 3869 | 3870 | 3867 | 654 | 3145 | 3146 | 2369 | 2541 | 2936 | 2935 | 1422 | 2371 | 2372 | 731 | 2373 | 3658 | 3581 | 3582 | 3583 | 3584 | 3799 | 3576 | 3663 | 2377 | 708 | 1877 | 2365 | 2366 | 716 | 840 | 2380 | 1697 | 2675 | 2676 | 877 | 3022 | 3021 | 3700 | 1878 | 2384 | 2385 | 2386 | 2387 | 2388 | 664 | 2770 | 2771 | 3270 | 1407 | 2389 | 2555 | 525 | 978 | 2397 | 1658 | 1882 | 1659 | 860 | 2748 | 1567 | 2402 | 2403 | 2404 | 2749 | 1018 | 2726 | 2727 | 1084 | 2405 | 3537 | 3534 | 1883 | 671 | 2411 | 2413 | 2414 | 3176 | 889 | 2921 | 2922 | 3125 | 3126 | 962 | 2415 | 1001 | 3195 | 3196 | 567 | 3107 | 3108 | 2420 | 2421 | 3399 | 1120 | 3163 | 3164 | 1710 | 563 | 2586 | 2587 | 2514 | 3058 | 3059 | 3223 | 915 | 1889 | 1890 | 2610 | 2611 | 3392 | 3535 | 2423 | 2422 | 514 | 3277 | 1891 | 2643 | 3344 | 3536 | 1755 | 1002 | 3395 | 3361 | 2425 | 2426 | 1563 | 1518 | 3180 | 3259 | 1487 | 3398 | 1894 | 1895 | 2427 | 3451 | 574 | 2428 | 2639 | 2816 | 944 | 2817 | 3795 | 967 | 2984 | 3405 | 2429 | 3670 | 3323 | 3120 | 3122 | 3121 | 646 | 2934 | 2933 | 918 | 2438 | 2352 | 2353 | 1003 | 2441 | 3502 | 3609 | 2445 | 3686 | 1025 | 1904 | 1905 | 2446 | 2447 | 3816 | 590 | 2640 | 1906 | 1907 | 3701 | 3706 | 3273 | 2452 | 988 | 2755 | 2756 | 3575 | 1105 | 2456 | 2455 | 584 | 1510 | 2430 | 2457 | 3618 | 3620 | 3619 | 1685 | 2459 | 1664 | 1162 | 1727 | 1918 | 2644 | 638 | 2464 | 3461 | 1937 | 1936 | 1938 | 1939 | 2677 | 2678 | 991 | 3791 | 3783 | 1940 | 3589 | 851 | 1946 | 1947 | 3474 | 1897 | 2544 | 1951 | 2546 | 1899 | 3819 | 171 | 3818 | 1898 | 1950 | 2545 | 3817 | 3182 | 562 | 1955 | 1956 | 2899 | 2900 | 3847 | 2276 | 1958 | 1961 | 2941 | 2942 | 2943 | 717 | 1962 | 1963 | 685 | 2052 | 2053 | 3639 | 2553 | 2554 | 3187 | 3694 | 3692 | 3654 | 3653 | 1967 | 2592 | 1968 | 2396 | 2375 | 1876 | 2374 | 3671 | 3184 | 3573 | 3413 | 3338 | 886 | 2476 | 2477 | 842 | 3105 | 3106 | 3001 | 3003 | 3002 | 2700 | 3019 | 1109 | 3018 | 2701 | 3020 | 3158 | 3159 | 3160 | 3231 | 3372 | 1979 | 3150 | 3151 | 3152 | 855 | 2940 | 2939 | 2930 | 2931 | 2932 | 830 | 1730 | 2616 | 1989 | 1315 | 2617 | 1511 | 2593 | 3082 | 3083 | 3084 | 3661 | 729 | 3085 | 3086 | 3597 | 2746 | 2747 | 2494 | 2495 | 854 | 2929 | 1992 | 1993 | 1994 | 1711 | 3242 | 3245 | 3239 | 3241 | 3240 | 3243 | 3238 | 3246 | 3244 | 3247 | 3248 | 3249 | 1502 | 1995 | 1996 | 1997 | 3532 | 3533 | 2821 | 3679 | 740 | 2466 | 2467 | 3362 | 2691 | 2004 | 3410 | 3513 | 3666 | 863 | 2007 | 2481 | 2482 | 3342 | 3697 | 3696 | 1781 | 1626 | 1087 | 2009 | 2010 | 2011 | 1712 | 2735 | 2736 | 3041 | 3042 | 1752 | 1082 | 2381 | 2674 | 2483 | 2014 | 2015 | 2488 | 2489 | 2655 | 108 | 2268 | 2269 | 1043 | 2485 | 3594 | 3595 | 1044 | 2629 | 1005 | 2019 | 2018 | 3408 | 2752 | 2753 | 2754 | 3737 | 660 | 2486 | 1601 | 2487 | 1064 | 2067 | 2068 | 905 | 3336 | 3481 | 1621 | 2072 | 2073 | 3603 | 3751 | 3790 | 2075 | 3186 | 3509 | 1512 | 2077 | 2078 | 2080 | 2079 | 2081 | 3559 | 3478 | 2082 | 2083 | 1735 | 2046 | 738 | 2382 | 2383 | 3412 | 3411 | 1635 | 1634 | 2667 | 2668 | 2091 | 2096 | 2097 | 3538 | 3539 | 3540 | 2101 | 3333 | 2103 | 2104 | 3153 | 3154 | 3155 | 3284 | 2106 | 2107 | 2108 | 3648 | 686 | 2114 | 683 | 2116 | 421 | 2594 | 577 | 2624 | 3823 | 3822 | 807 | 568 | 2117 | 2214 | 1706 | 2118 | 3730 | 2215 | 3728 | 3729 | 100 | 3216 | 3220 | 2120 | 2502 | 2503 | 2125 | 2126 | 867 | 2919 | 2920 | 3207 | 3188 | 2133 | 705 | 2134 | 2137 | 2138 | 3757 | 1028 | 2737 | 2738 | 2141 | 2140 | 1676 | 3260 | 3698 | 2151 | 2152 | 875 | 2969 | 3208 | 3566 | 3789 | 3396 | 3360 | 3785 | 1636 | 3485 | 3486 | 3675 | 1533 | 3484 | 2623 | 1587 | 3286 | 3285 | 3183 | 1668 | 3710 | 3742 | 2657 | 1578 | 1617 | 3213 | 1942 | 1943 | 1944 | 2159 | 2160 | 3324 | 3326 | 3325 | 3217 | 1696 | 3492 | 3516 | 1125 | 2656 | 3447 | 3363 | 3054 | 3327 | 954 | 3024 | 2509 | 2161 | 2162 | 3772 | 928 | 715 | 246 | 3874 | 3608 | 942 | 894 | 885 | 822 | 969 | 1038 | 604 | 895 | 1037 | 869 | 1077 | 959 | 976 | 862 | 1104 | 1000 | 897 | 222 | 838 | 960 | 609 | 585 | 899 | 926 | 608 | 887 | 666 | 835 | 900 | 1050 | 1107 | 936 | 258 | 1027 | 59 | 1029 | 982 | 983 | 625 | 1079 | 1047 | 881 | 914 | 985 | 1014 | 597 | 583 | 929 | 1015 | 1094 | 616 | 1072 | 1081 | 817 | 874 | 818 | 999 | 882 | 1024 | 821 | 801 | 825 | 1030 | 1052 | 1048 | 891 | 865 | 852 | 864 | 1083 | 916 | 925 | 994 | 996 | 1036 | 846 | 1041 | 917 | 554 | 938 | 1085 | 850 | 970 | 980 | 950 | 1004 | 606 | 582 | 819 | 820 | 620 | 989 | 935 | 866 | 990 | 843 | 1042 | 973 | 957 | 904 | 610 | 1031 | 828 | 1026 | 804 | 815 | 1040 | 1063 | 1065 | 1034 | 796 | 594 | 1066 | 1009 | 930 | 1056 | 829 | 848 | 943 | 1076 | 576 | 834 | 884

URL: Case Study: Testing a Native Clay Using Insight-Live.com

Click the link below to go to this page

https://insight-live.com/insight/help/It+Starts+With+a+Lump+of+Clay-433.html

Related Information

Click here for case-studies of Insight-Live fixing problems


Insight-live help button

This picture has its own page with more detail, click here to see it.

You will see examples of replacing unavailable materials (especially frits), fixing various issues (e.g. running, crazing, settling), making them melt more, adjusting matteness, etc. Insight-Live has an extensive help system (the round blue icon on the left) that also deals with fixing real-world problems and understanding glazes and clay bodies.

Step 11: 40, 50, 70, 100 mesh oversize particles (clockwise)


Micro photographs of clay particles

This picture has its own page with more detail, click here to see it.

These photos were taken by an iPhone 13 at 1-inch distance. They are the residue on each of the four sieves (remember I already sieved the material through 30 mesh, the top sieve thus represents the 30-40 mesh fraction). From these, it appears that the particulate in the clay is mostly rounded quartz particles. Their presence explains the sandy feel of the material during throwing (strangely, round particles generally feel sandier than angular ones). The reason it was difficult to wet-sieve through 30 mesh is that these rounded particles must be clogging the screen. It is a safe assumption that if it was tested down to 325 mesh, the percentage of quartz sand on each sieve would continue to increase. Because these particles are present at all sizes measured, the same clogging issue would occur at any mesh size. The presence of so many quartz grains also means it would be just about impossible to grind this finer than 30 mesh in a hammer mill. This being said, the presence of so many quartz particles likely means glazes will fit well (or possibly even shiver), it will have good drying performance and the plastic material should dewater quickly.

How to decide what temperature to fire this clay at?


Test bars of a terra cotta clay fired from cone 06-8

This picture has its own page with more detail, click here to see it.

This is an extreme example of firing a clay at many temperatures to get a wide-angle view of it. These SHAB test bars characterize a terra cotta body, L4170B. While it has a wide firing range, its "practical firing window" is much narrower than these fired bars and the graph suggest. On paper, cone 5 hits zero porosity. And, in hand, the bar feels like a porcelain. But ware warps during firing, and transparent glazes will be completely clouded with bubbles (when pieces are glazed inside and out). What about cone 3? Its numbers put it in stoneware territory, watertight. But decomposition gases still bubble glazes! Cone 2? Much better; it has below 4% porosity (any fitted glaze will make it watertight), below 6% fired shrinkage, still very strong. But there are still issues: Accidental overfiring drastically darkens the color. Low-fire commercial glazes may not work at cone 2. How about cone 02? This is a sweet spot. This body has only 6% porosity (compared to the 11% of cone 04). Most low-fire cone 06-04 glazes are still fine at cone 02. And glaze bubble-clouding is minimal. What if you must fire this at cone 04? Pieces will be "sponges" with 11% porosity, shrinking only 2% (for low density, poor strength). There is another advantage of firing as high as possible: Glazes and engobes bond better. An example of a low-fire transparent base that works fine on this up to cone 2 is G1916Q.

Step-by-step how to test and evaluate a new native clay


Two lumps of raw clay dug straight out of a hill

This picture has its own page with more detail, click here to see it.

"It Starts With a Lump of Clay", a step-by-step Insight-Live.com tutorial (from its help system and the link below) on how to document every step (in an account at insight-live.com) of testing a raw clay. You will learn about drying shrinkage, drying performance, particle size distribution, plasticity, firing shrinkage, fired porosity, fired color, soluble salt content, fired strength, etc. We will not just observe these properties, but measure them. In doing so we will characterize the material. We will answer simple questions about how the material forms, dries and fires across a range of temperatures. In doing the testing I will be generating a lot of data. No single factor is more intimidating to new technicians than what to do with this data, how and where to store it, how it can be searched, learned from, compared.

Testing your own native clays is easier than you think


Simple tests being done on a found clay

This picture has its own page with more detail, click here to see it.

Some simple equipment is all you need. You can do practical tests to characterize a local clay in your own studio or workshop (e.g. our SHAB test, DFAC test, SIEV test, LDW test). You need a gram scale (preferably accurate to 0.01g) and a set of callipers (check Amazon.com). Some metal sieves (search "Tyler Sieves" on Ebay). A stamp to mark samples with code and specimen numbers. A plaster table or slab. A propeller mixer. And, of course, a test kiln. And you need a place to put all the measurement data collected and learn from it (e.g. an account at insight-live.com).

Precrush raw lump clay:

Use a large wooden rolling pin


This picture has its own page with more detail, click here to see it.

These two clays arrived for testing and characterization, with lumps up to 1 inch. After making sure the material is completely dry, I spread out about 1kg on the concrete floor and then roll it using a large rolling pin. This effectively breaks the lumps. If I just keep rolling the whole mass thins more and more and the lumps get smaller and smaller (making them much easier to slake). Another benefit is that rocks are located, since the rolling pin is unable to break them. Finally, the homogeneity of the material is clearly visible. In these two clays, it is clear that the left one is homogeneous, all of the lumps being the same grey material (the right one looks more like overburden than useable clay, likely not worthy of further investigation).

Links

Tests Drying Factor
The DFAC Drying Factor test visually displays a plastic clay's response to very uneven drying. It is beneficial to show the relative drying performance of different clays.
Tests LOI/Density/Water Content
LDW LOI, density and water content test procedure for plastic clay bodies and porcelains
Tests Sieve Analysis 35-325 Wet
A measure of particle size distribution by washing a powdered or slaked sample through a series of successively finer sieves
Articles Formulating a body using clays native to your area
Being able to mix your own clay body and glaze from native materials might seem ridiculous, yet Covid-19 taught us about the need for independence.
Articles How to Find and Test Your Own Native Clays
Some of the key tests needed to really understand what a clay is and what it can be used for can be done with inexpensive equipment and simple procedures. These practical tests can give you a better picture than a data sheet full of numbers.
Glossary Digitalfire Insight-Live
A cloud-hosted ceramics-targeted LIMS (lab info management system). It does glaze chemistry and physical testing the “Digitalfire way”. For technicians, educators, potters and hobbyists.
Glossary Particle Size Distribution
Knowing the distribution of particle sizes in a ceramic material is often very important in assessing its function and suitability for an application.
Glossary Drying Shrinkage
Clays used in ceramics shrink when they dry because of particle packing that occurs as inter-particle water evaporates. Excessive or uneven shrinkage causes cracks.
Glossary Firing Shrinkage
During drying, clay particles draw together and shrinkage occurs. During firing the matrix densifies and shrinkage continues. More vitreous bodies shrink more.
Glossary Physical Testing
In ceramics, glazes, engobes and bodies have chemistries and physics. Your formulation and quality control most likely need to focus on the physical properties.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.

Got a Question?

Buy me a coffee and we can talk

 