1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Feldspar

Oxide Analysis Formula Tolerance
K2O 16.92% 1.00
Al2O3 18.32% 1.00
SiO2 64.76% 6.00
Oxide Weight 556.74
Formula Weight 556.74

Notes

Theoretically speaking, the term 'feldspar' refers to a family of minerals with a specific crystalline presence. However actual feldspar powders are made from crushed crystalline rock containing a mixture of aluminum silicates of sodium and potassium (with minor amounts of lithium or calcium). They normally contain 10-15% alkali (K2O, Na2O) and melt well at medium to high temperatures and are an economic source of flux. Commercially available feldspars tend to predominate in one specific mineral kind with lesser amounts of another and traces of others. Manufacturers can be found around the world and they usually do a good job of delivering uniform and clean products when one considers that feldspar deposits vary widely in composition and contain many impurities. Large quantities of feldspar are used in non-ceramic industry (e.g. cement, agri).

In many countries feldspar companies draw upon the same mine year and year, marketing a brand name product that gains wide acceptance. In other countries (e.g. India) large feldspar suppliers do not even have mines, they buy raw product according to the chemistry and blend from different sources to achieve a specific product. Over time they change suppliers but through careful quality control, their ceramic manufacturing customers often do not realize their feldspar is coming from different sources with different shipments. Increasingly customers are connecting with suppliers on other continents, not infrequently this has led to misunderstandings and delivery of bad or variable product.

Generally, high potash feldspars are employed in bodies and promote vitrification by forming a glassy phase that 'cements' more refractory particles together and triggers the formation of mullite from clay mineral. It is typical to see about 25% feldspar in cone 10 vitreous bodies (1300C) and 35% at cone 6 (1200C), although porcelains may have a little more. Much below 1200C feldspar will not produce a vitreous body. Manufacturers often employ feldspar percentages inappropriate to their situations and other materials (like silica sand, alumina, extra quartz) are added to compensate. It is important to test the porosity and fired shrinkage of your body at temperatures above and below your production firing (e.g. -30, -60, -90, +30, +60, +90). This will tell you where you are on the porosity and shrinkage curves (it is not good to be near or on the down-slope of the firing shrinkage or up-slope of the porosity). You can organize this testing in your account at insight-live.com.

In glazes, feldspar promotes melting at medium and high temperatures (feldspars are the primary ingredient in most high-temperature raw glazes). Sodium feldspars are most common and used mainly as a source of alkalis. Feldspars are mineral compounds of silica, alumina and fluxes and are among the relatively few insoluble sources of K2O, Na2O and Li2O. No other raw material is closer to being a complete stoneware glaze on its own than feldspar. Since feldspars contain a complex mix of oxides, ceramic chemistry calculations are needed to 'juggle' a recipe to achieve the desired balance of fluxing oxides with alumina and silica and to control the high thermal expansion that they impart.

Many feldspars begin to melt around 2100F (1150C) and make good glaze bases because they contribute alumina and silica in forms that participate well in the melt. Feldspars tend to work well in fast-fire high-temperature glazes because they remain relatively inert until the later stages of firing.

Geologists see feldspar as a mineral and classify feldspars mainly as albite, microcline, orthoclase and anorthite. However, for use in glazes, we can view feldspars as 'warehouses of oxides' (e.g. because they supply K2O, Na2O, Al2O3 and SiO2 to the glaze melt).

Alert
'Flux-saturated' glazes with high feldspar contents tend to be chemically unbalanced and thus make poor bases for functional ware, especially for glaze containing metallic color oxides (the glazes can be soft, leachable, crazed, oxidizable). High feldspar can contribute to a high surface tension in the glaze melt and may lead to high bubble population (producing milkiness in the fired matrix). Stoneware glazes using large amounts of feldspar as a flux almost always craze because high-expansion sodium and potassium predominate. High feldspar glazes often lack clay content and thus do not suspend well, they settle in a hard layer on the bottom of the container and dry to a powdery surface on ware. In fact, thousands of potters are using feldspar saturated glazes and living with many problems without being aware of the cause.

Related Information

Stockpile of crude feldspar from MGK Minerals (India) deposit


This picture has its own page with more detail, click here to see it.

Closeup of feldspar deposit in the MGK Minerals quarry in India


This picture has its own page with more detail, click here to see it.

Feldspars, the primary high temperature flux, melt less than you think.


Feldspar melt flows at cone 8 and 11

This picture has its own page with more detail, click here to see it.

Our melt fluidity tester is being used to compare cone 8 melt fluidities of Custer, G-200 and i-Minerals high soda and high potassium feldspars. Notice how little the pure materials are moving (bottom), even though they are fired to cone 11. In addition, the sodium feldspars move better than the potassium ones. But feldspars do their real fluxing work when they can interact with other materials. As a demonstration of that, note how well they flow with only 10% frit added (top), even though fired three cones lower.

A soda feldspar applied like at glaze at cone 4-7


Feldspar as a glaze on porcelain tiles

This picture has its own page with more detail, click here to see it.

This is pure soda feldspar (Minspar 200) fired like a glaze at cone 4, 5, 6 and 7 on porcelainous stoneware tiles. The bottom samples are balls that have melted down at cone 7 and 8 (although they appear to be well melted they exhibit no movement in a melt fluidity test. Notice there is no melting at all at cone 4. Also, serious crazing is highlighted with ink on the cone 6 sample (it is also happening at cone 5 and 7). Feldspars have high KNaO, that means they have high thermal expansions. That is why high-feldspar glazes almost always craze. Since feldspar is barely melting at cone 6 it is not possible to make a functional cone 6 glaze that only uses feldspar as the flux (boron, lithia or zinc are also needed).

Craze city: Pure Feldspar and Nepheline Syenite


This picture has its own page with more detail, click here to see it.

These pure material powders were applied to bisque as slurries, suspended by gelling with Epsom salts, and fired at cone 10R. On the left is Custer feldspar on a Grolleg porcelain (P700); on the right is Covia nepheline syenite on a whiteware body (P600).

Feldspars and nepheline syenite supply large amounts of K2O and Na2O, oxides having very high thermal-expansion contributions in glaze chemistry. When these materials are melted essentially by themselves, the resulting glasses have very high thermal expansion relative to typical ceramic bodies - thus the spectacular crazing seen here. Glaze recipes containing high percentages of them can likewise be prone to crazing unless enough lower-expansion oxides, especially SiO2, Al2O3 and MgO, are present.

This feldspar melts by itself to be a glaze, but crazes badly


This picture has its own page with more detail, click here to see it.

Pure MinSpar feldspar fired at cone 6 on Plainsman M370 porcelain. Although it is melting, the crazing is extreme! And expected. Feldspars contain a high percentage of K2O and Na2O (KNaO), these two oxides have the highest thermal expansion of any oxide. By far! Thus, glazes high in feldspar (e.g. 50%) are likely to craze. Using a little glaze chemistry, it is often possible to substitute some of the KNaO for another fluxing oxide having a lower thermal expansion.

Start glaze chemistry by learning when you don't need it!

A high feldspar glaze is a good example


A runny, amber, crazed glaze

This picture has its own page with more detail, click here to see it.

This reduction celadon is crazing badly. Why? Its chemistry is dominated by feldspar, which supplies lots of K2O and Na2O fluxes. Scores of recipes being traded online contain 50% or more feldspar; they benefit from these powerful fluxes but inherit their high thermal expansion (COE). Many work only because the body happens to have sufficiently high expansion - often aided by significant residual quartz.

Crazing is more than a cosmetic problem in functional pieces. It reduces ware strength and durability, can compromise food safety and turn into a customer complaint. Let's fix it, starting without chemistry:

Getting the feldspar percentage right in an iron reduction clay body


Iron reduction clay body surface character

This picture has its own page with more detail, click here to see it.

We are trying to achieve a body sufficiently vitreous for functional ware but open enough to still have the characteristic variegated patching of light and dark brown (with reduction iron speck of course). Our base recipe is a two-part mix of red and buff fireclay. Mugs #1 and #2 have 12% Custer feldspar but #2 has more of the white clay (it’s more refractory and more plastic - so #2 has a porosity of 3.5% while #1 has 2.8%). #3 has the same clay mix as #2 but it uses 12% Nepheline Syenite - it’s greater fluxing power has turned the color a solid brown (and dropped porosity to 1.5%). The next step: We will target 3% porosity in #3 using a reduced percentage of Nepheline, likely about 9%. We have depended on 100% clay mixes in the past and the body has suffered variations in density (as measured by our SHAB test) and has seldom hit the 3% porosity target, having feldspar in the recipe will enable accurately controlling it in future (so we are more comfortable recommending it for light duty functional ware).

Feldspar from Okene, Koji, Nigera


This picture has its own page with more detail, click here to see it.

High feldspar glazes craze on functional:

Don't put up with it. Fix them.


This picture has its own page with more detail, click here to see it.

This glaze, "Bamboo Cone 10%", contains 50% potash feldspar, so it certainly qualifies as a high-feldspar glaze. K2O and Na2O are thus oversupplied. They have the highest thermal expansions of all oxides, by far. These are needed and valuable, but when grossly oversupplied the result is crazing. This glaze used to work on this body, H550. The previous version of H550 was firing near the bloating point of the body, about 1% porosity, so the recipe had to be changed to provide more margin for error. The new recipe has a more practical 2.0-2.5% porosity; it has no danger of bloating or warping and still has excellent maturity and strength. This glaze was crazing before, and pieces did not leak because the body was dense enough - so they were still watertight. But now it does not work. The solution is to do something that should have been done before: Use a silky matte base recipe that does not craze. I recommend the G2571A base (below right) - the Zircopax, rutile, and iron oxide in the original can be added to it instead.

Which is the champion melter of American/Canadian feldspars?


Feldspars melting

This picture has its own page with more detail, click here to see it.

Feldspars are employed in glaze recipes as melters. So comparing their melt fluidities should be helpful in deciding if one can substitute for another (of course, if possible, a soda-predominant feldspar should be substituted for another soda spar). Feldspars don't melt alone at cone 6 (2200F) so we mixed each with 15% Ferro Frit 3195 (we consider a feldspar a material that sources KNaO). Nepheline Syenite, this is A270, is the champion melter here. Other similar ones can be spotted easily. In the end, degree of melt is a valid consideration in determining if one feldspar is a viable substitute for another in a recipe. Even if the feldspar you want to substitute does not melt as much a little frit can be added to the recipe to make up for the difference (e.g. 3-5%).

Links

Glossary Feldspar Glazes
Feldspar is a natural mineral that, by itself, is the most similar to a high temperature stoneware glaze. Thus it is common to see alot of it in glaze recipes. Actually, too much.
Glossary Crackle glaze
Crackle glazes have a crack pattern that is a product of thermal expansion mismatch between body and glaze. They are not suitable on functional ware.
Materials Kona F-4 Feldspar
Materials Minspar 200
Materials G-200 2R Feldspar
Materials M-200 Feldespato
Materials Pegmatite
Materials Kaolin A
Materials Feldspath ICE 10
Materials Nepheline Syenite
Materials Spodumene
Spodumene is a lithium sourcing feldspar, an alternative to lithium carbonate to supply Li2O to ceramic glazes. Contains up to about 8% Li2O.
Materials Calcium Feldspar
Materials Potash Feldspar
A feldspar having a KNaO content that predominates in potassium.
Materials Soda Feldspar
A feldspar having a KNaO content that predominates in sodium.
Materials Custer Feldspar (pre-2000)
The most common potash feldspar used in ceramics in North America. It was a standard for many decades but is no longer available.
Materials Ferro Frit 3110
High sodium, high thermal expansion low boron frit. A super-feldspar in clay bodies. Melts at very low temperatures. Useful to make crackle glazes.
Materials Nepheline Syenite Norwegian
Media A Broken Glaze Meets Insight-Live and a Magic Material
Use Insight-Live.com to do major surgery on a feldspar saturated cone 10R glaze recipe with multiple issues: blistering, pinholing, crazing, settling, dusting and possibly leaching!
Media Mica and Feldspar Mine of MGK Minerals
URLs http://studiopotter.org/pdfs/Sohng%20pps84-89.pdf
Article about cristobalite in clay bodies
URLs https://www.youtube.com/watch?v=FVUuhjnjAoA
German potter Cornelius Breymann investigates limit formulas, eutectics
On this Youtube video Cornelius will take you on a slow and deliberate journey. If you stick with him you will discover how, by industrious blending of feldspar, calcium carbonate and silica we can see what ratios of CaO, SiO2 and Al2O3 (and the materials sourcing them) produce a well-melted high temperature glaze. You will see how the process demonstrates where feldspar comes up short as a glaze by itself and what it needs to be one. And you will see the CaO:SiO2:Al2O3 eutectic demonstrated.
URLs http://en.wikipedia.org/wiki/Feldspar
Wikipedia Feldspar Page
URLs http://en.wikipedia.org/wiki/Feldspar
Feldspar at Wikipedia
Articles Are Your Glazes Food Safe or are They Leachable?
Many potters do not think about leaching, but times are changing. What is the chemistry of stability? There are simple ways to check for leaching, and fix crazing.
Articles Formulating a Porcelain
The principles behind formulating a porcelain are quite simple. You just need to know the purpose of each material, a starting recipe and a testing regimen.
Articles Crazing in Stoneware Glazes: Treating the Causes, Not the Symptoms
Band-aid solutions to crazing are often recommended by authors, but these do not get at the root cause of the problem, a thermal expansion mismatch between glaze and body.
Articles Is Your Fired Ware Safe?
Glazed ware can be a safety hazard to end users because it may leach metals into food and drink, it could harbor bacteria and it could flake of in knife-edged pieces.
Articles Bringing Out the Big Guns in Craze Control: MgO (G1215U)
MgO is the secret weapon of craze control. If your application can tolerate it you can create a cone 6 glaze of very low thermal expansion that is very resistant to crazing.
Articles A Low Cost Tester of Glaze Melt Fluidity
Use this novel device to compare the melt fluidity of glazes and materials. Simple physical observations of the results provide a better understanding of the fired properties of your glaze (and problems you did not see before).
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.
Typecodes Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials.
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.
Hazards Feldspar
Feldspars are abundant and varied in nature. They contain small amounts of quartz (while nepheline syenite does not).
Oxides KNaO - Potassium/Sodium Oxides
Oxides SiO2 - Silicon Dioxide, Silica
Oxides Li2O - Lithium Oxide, Lithia
Oxides Na2O - Sodium Oxide, Soda
Oxides Al2O3 - Aluminum Oxide, Alumina
Troubles Powdering, Cracking and Settling Glazes
Powdering and dusting glazes are difficult and a dust hazard. Shrinking and cracking glazes fall off and crawl. The cause is the wrong amount or type of clay.
Troubles Glaze Crazing
Ask the right questions to analyse the real cause of glaze crazing. Do not just treat the symptoms, the real cause is thermal expansion mismatch with the body.

Mechanisms

Body MaturityFeldspar is the most important body flux for cone 2+. Many clays and other body materials contain feldspar. The classic cone 10 porcelain recipe is 25% each of feldspar, ball clay, silica and kaolin.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 