1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Nepheline Syenite Norwegian

Alternate Names: North Cape Nepheline Syenite, Spectrum N500

Description: Norwegian Nepheline Syenite

Oxide Analysis Formula Tolerance
K2O 8.80% 0.41
SiO2 57.20% 4.22
Al2O3 24.40% 1.06
Na2O 8.20% 0.59
Fe2O3 0.10% -
TiO2 0.10% 0.01
LOI 1.00%n/a
Oxide Weight 437.80
Formula Weight 442.22

Notes

North Cape nepheline syenite is produced in the north of Norway, near the Alta fjord within the Arctic circle. This has a much higher K2O (and lower Na2O) than the Canadian material.

The analysis on the Sibelco data page likely has an error in the SiO2, we have changed it from 53.2 to 57.2.

May 2025: The Norwegian NS45 appears to be no longer available. They have substituted a new series, apparently mined in Sweden but processed in Thailand. The chemistry is very similar (56% SiO2, 24% Al2O3, 8% Na2O, 9% K2O, 2% CaO, 0.1% Fe2O3).

Related Information

Links

Materials Feldspar
In ceramics, feldspars are used in glazes and clay bodies. They vitrify stonewares and porcelains. They supply KNaO flux to glazes to help them melt.
Materials Nepheline Syenite
URLs https://digitalfire.com/4sight/datasheets/NephelineSDataSheet.pdf
Sibelco Nepheline S Thailand Data Sheet
This is mined in Sweden and processed in Thailand. It is the successor to Norwegian Nepheline.
URLs https://www.sibelco.com/en/materials/nepheline-syenite
Sibelco Nepheline Syenite page
They claim their nepheline syenite is a quartz-free aluminium silicate. It primarily comprises nepheline, microcline and albite. Because of its extremely low melting point and high alumina content, Sibelco nepheline syenite is used as a flux in ceramics, to lower melting temperatures in glass, and as a functional filler in coatings and polymers.
URLs http://www.handbookofmineralogy.org/pdfs/Nepheline.pdf
Nepheline mineralogy
URLs http://en.wikipedia.org/wiki/Nepheline
Nepheline at Wikipedia
Hazards Feldspar
Feldspars are abundant and varied in nature. They contain small amounts of quartz (while nepheline syenite does not).
Typecodes Materials used in Denmark
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.