Alternate Names: Calcined Rutile, Light Rutile, Rutile Ceramic
Formula: TiO2
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| TiO2 | 75.00% | 4.21 | |
| ZrO | 0.60% | 0.03 | |
| SiO2 | 0.90% | 0.07 | |
| Fe2O3 | 0.50% | 0.01 | |
| K2O | 21.00% | 1.00 | |
| Oxide Weight | 439.60 | ||
| Formula Weight | 439.60 | ||
Because it is ground to minus 325 mesh and calcined, ceramic rutile powder is a light brown (vs. the black raw granular material). It is the recommended type for use in ceramic glazes since it will not produce gases of decomposition.
The theoretical chemistry of pure rutile is TiO2 (however no mineral deposit of rutile is pure). Good quality ores are blended to achieve consistency, lower quality ones can be processed in furnaces to increase purity. However, rutile is a feedstock to make potassium titanate, the rutile commonly used for ceramics in North America (from TAMCeramics.com). Its original container bags are labelled "Weld Rod Titanate" (for use in welding rods). Since they are adding K2O (as a flux) this is a furnace-processed material whose purity and quality are tuned and maintained. The potassium is not a problem in ceramics, it is a flux found in all glazes containing feldspar. The high consistency offered by this grade makes it preferred in ceramics (over pure rutile).

This picture has its own page with more detail, click here to see it.
This bag is very small, this material is very dense and heavy. The primary use of this material is obvious: For making welding rods. We can thus assume it will continue to be abundantly available for ceramics. Notice the bag bottom is marked "Ceramic Rutile" (with a batch number). Why would a product intended for making welding rods be used in ceramics? The answer is very interesting.

This picture has its own page with more detail, click here to see it.
Left: GA6-C rutile blue glaze on a brown stoneware. The 4% ceramic rutile powder gives the blue variegated effect. Right: We ball-milled our granular rutile and then screened it down to 325 mesh and put that into the same glaze. The results are the same. So if any of your rutile glazes ever lose this effect with a new supply of the material the cause could be that it has not been milled sufficiently fine. Finer rutile powders are browner in color.

This picture has its own page with more detail, click here to see it.
Yes, the granular and powdered grades of pure rutile are the same material. But, for producers, the milling process it is very difficult because the raw mineral is so hard. Commercial ceramic grade powder is minus 325 mesh, the companies doing this obviously have very good grinding equipment. They also have patience because even in this efficient porcelain ball mill, 90 minutes was only enough to get 50% to minus 325 mesh! The color of the powder is a good indication of its quality, the finer the grind the lighter tan it will be. That means you can use the color to gauge the mesh size. And, if you have a ball mill you can milled it more if needed.

This picture has its own page with more detail, click here to see it.
Rutile variegates glaze surfaces. But it also opacifies at higher percentages. The blue effect is a product of crystallization that occurs during cooling, it is thus dependent on a slower cooling cycle, especially above 1400F. This is GA6-C Alberta Slip glaze with 4, 5 and 6% rutile. At 6% the rutile crystallization has advanced to the point of completely opacifying the glaze. At 5% the blue is still strong, even on a buff burning body. The loss of color occurs suddenly, somewhere between 5 and 6 percent. Rutile chemistry varies from batch to batch. The blue develops differently on different bodies. So do you want to play "at the edge", with 5% in the glaze, in view of these other factors and the finicky firing curve needed. Change in any of which could push it into the blueless zone?

This picture has its own page with more detail, click here to see it.
The 80:20 GA6-A Alberta Slip base becomes oatmeal-like when oversaturated with rutile and/or titanium (left: 6% rutile + 3% titanium dioxide; right: 4% rutile + 2% titanium dioxide). The rough surface results from excessive crystallization of titanium-bearing phases from the melt during cooling. It is unpleasant to touch, readily shows cutlery marking and is less desirable for functional surfaces. In glazes of this type, rutile additions above about 4% can become increasingly difficult to keep smooth and consistent. Crystallization, rather than phase separation, increasingly dominates the variegation mechanism.
One way of avoiding problems is staying below the tipping point, keeping the percentage as low as possible while still getting the desired variegation (of course, that will vary depending on the melt fluidity of the glaze and kiln cooling). Surprisingly, making the glaze more fluid does not necessarily solve the problem. Greater melt fluidity increases ion mobility and can actually promote crystal growth during cooling, producing an even rougher surface.

This picture has its own page with more detail, click here to see it.
This is a common problem with these glazes. The visual effect is very compelling but also punishing! Potters experiment with higher bisque firing and soaking during bisque. They try cleaner clay bodies. They employ long hold periods at temperature in the glaze firing. But the problem persists. The solution is actually simpler. These glazes have a high melt fluidity and enough surface tension to hold a bubble static during soaks at temperature (no matter how long you hold it). It is better to cool the kiln somewhat (perhaps 100F) and soak at that temperature. Why? Because the increasing viscosity of the melt overcomes the surface tension that maintains the bubbles. You may need to cool more or less than 100 degrees, but start with that.

This picture has its own page with more detail, click here to see it.
These mugs are Plainsman H450 fired at cone 10R. Both have a black engobe (L3954N) applied to the insides and half way down the outside during leather hard stage (the insides are glazed with Ravenscrag silky matte and G1947U over the black engobe). The bamboo glazes can thus be seen over the black (upper half) and the raw buff body (lower). The bamboo glaze on the left has 1% iron added to the base G2571A recipe. The one on the right has 3.5% powdered rutile and 10% zircopax added.

This picture has its own page with more detail, click here to see it.
These are GA6-C Alberta Slip floating blue (left), AMACO Potter's Choice PC-20 Blue Rutile (center), GR6-M Ravenscrag floating blue (right). The clay is M390. The firing is cone 6, the schedule is C6DHSC (drop-and-hold, slow cool). All of these recipes are descendants and improvements of the 50-year-old original G2826R floating blue. The inside glaze on these mugs is GA6-B. The two on the left develop the blue color because of the slow cool, the one on the right works on fast-cool (because it contains cobalt). Remember, floating blue is a rutile blue glaze, as such it works best on dark-burning bodies.

This picture has its own page with more detail, click here to see it.
A closeup of a cone 10R rutile blue (it is highlighted in the video: A Broken Glaze Meets Insight-Live and a Magic Material). Beautiful glazes like this, especially rutile blues, often have serious issues (like blistering, crazing), but they can be fixed.

This picture has its own page with more detail, click here to see it.
These metal oxides have been mixed with 50% Ferro frit 3134 and fired to cone 6 oxidation. Chrome and rutile have not melted, copper and cobalt are extremely active melters, frothing and boiling. Cobalt and copper have crystallized during cooling. Manganese has formed an iridescent glass.

This picture has its own page with more detail, click here to see it.
2, 3, 4, 5% rutile added to an 80:20 mix of Alberta Slip:Frit 3134 at cone 6. This variegating mechanism of rutile is well-known among potters. Rutile can be added to many glazes to variegate existing color and opacification. If more rutile is added the surface turns an ugly yellow in a mass of titanium crystals.

This picture has its own page with more detail, click here to see it.
The glaze is a dolomite matte fired to cone 10R. High fire reduction is among the best processes to exploit the variegating magic of rutile.

This picture has its own page with more detail, click here to see it.
The glaze is G191T (a variation of G1916Q). Firing was cone 04 drop-and-hold with slow cool. Sometimes a raw colorant is advisable over a ceramic stain. At low temperatures stains are almost universal. But in this case, the orangey-yellow color that rutile produces merits further testing. On the red body (Plainsman L215) the color is barely perceptible, but on the light Buffstone body it is working well. The variations in thickness highlight contours better than what a stain would do.
| Materials |
Rutile
A raw TiO2-containing mineral used in ceramics to color and variegate glaze surfaces. |
| Materials |
Titanium Dioxide
A super white powder used in ceramic glazes to variegate, opacify and moderate color. |
| Materials |
Ilmenite
|
| Materials |
Ruflux 61
|
| Materials |
Granular Rutile
The same material as milled rutile, but ground only to granular size. |
| Glossary |
Rutile Blue Glazes
A type of ceramic glaze in which the surface variegates and crystallizes on cooling in the presence of titanium and iron (usually sourced by rutile) |
| URLs |
https://tamceramics.com/wp-content/uploads/2016/05/SDS-Rutile.pdf
Ruflux 61 rutile data sheet |
| Typecodes |
Colorant
Metallic based materials that impart fired color to glazes and bodies. |
| Typecodes |
Opacifier
Opacifiers are powders that turn transparent glazes opaque by various chemical and physical mechanisms (and combinations of mechanisms). |
| Typecodes |
Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk