1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Ilmenite

Alternate Names: Illmenite, Ferrous Titanate, Iron Titanate

Description: Iron & Titanium Oxide

Formula: FeTiO3 or FeO.TiO2

Oxide Analysis Formula Tolerance
TiO2 49.41% 1.00
FeO 50.59% 1.00
Oxide Weight 161.71
Formula Weight 161.71

Notes

Like rutile, ilmenite is quite variable in nature. Actually, more variable since it would likely come from the same deposit, it being the more iron-stained part. You can tell the difference between granular rutile and granular ilmenite by doing a smear test against an abrasive surface (i.e. an unglazed white tile). The rutile stains tan or brown, the ilmenite black or dark brown. Under a microscope the ilmenite will be an opaque black whereas the rutile crystals will be somewhat translucent or transparent.

Ilmenite can be used in small amounts (-1%) to produce dark brown specks in bodies and specialized glazes. It also is used in combination with rutile to develop characteristic rutile break glazes; it seeds crystals in titania glazes.

If your production depends on consistency of this material, consider testing each batch of this material received by mixing it with a boron frit and doing a GBMF test. Variations in chemistry will be immediately evident.

Related Information


This picture has its own page with more detail, click here to see it.

0.5% fine granular illmenite added to Ravenscrag cone 6 clear glossy white base glaze.


This picture has its own page with more detail, click here to see it.

An illmenite colored glaze (GR6-H) at cone 6 oxidation

Links

URLs http://en.wikipedia.org/wiki/Ilmenite
Illmenite at Wikipedia
Minerals Illmenite
Ilmenite is a black colored heavy ore of iron and titanium. It is closely related to rutile. Materia
Minerals Anorthosite
A plagioclase feldspar rock containing ilmenite.
Materials Granular Ilmenite
Materials Granular Rutile
The same material as milled rutile, but ground only to granular size.
Materials Hematite
Materials Rutile
A raw TiO2-containing mineral used in ceramics to color and variegate glaze surfaces.
Materials Ceramic Rutile
Rutile mineral ground to a very fine particle size (e.g. 325 mesh) contributes titanium and iron that colors and variegates ceramic glazes.
Typecodes Flux Source
Materials that source Na2O, K2O, Li2O, CaO, MgO and other fluxes but are not feldspars or frits. Remember that materials can be flux sources but also perform many other roles. For example, talc is a flux in high temperature glazes, but a matting agent in low temperatures ones. It can also be a flux, a filler and an expansion increaser in bodies.
Typecodes Generic Material
Generic materials are those with no brand name. Normally they are theoretical, the chemistry portrays what a specimen would be if it had no contamination. Generic materials are helpful in educational situations where students need to study material theory (later they graduate to dealing with real world materials). They are also helpful where the chemistry of an actual material is not known. Often the accuracy of calculations is sufficient using generic materials.
Hazards Titanium Dioxide Toxicology

Data

Hardness (Moh) 6.0
Frit Softening Point 1365C
Density (Specific Gravity) 4.80

Mechanisms

Glaze CrystallizationIlmenite seeds crystals in titania glazes.
Glaze VariegationIlmenite can be used with rutile to produce classic rutile-breaking glazes. Use up to 2% ilmenite.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://backup.digitalfire.com, All Rights Reserved
Privacy Policy